Goh, J. H., Seo, J. W., Park, H. S., and Park, H. M. (2026). "Bending creep performance of wood flooring composited with cork composite boards reinforced with metal, glass fiber, and carbon fiber using temperate and tropical wood species,"  BioResources 21(4), 11367–11379.

Abstract

This study investigated the bending creep performance of cork composite wood floorings. The cork composite wood floorings consisted of two temperate species (tulip tree and larch) and two tropical species (teak and merbau) as the face layer, and a cork board reinforced with metal, glass fiber, or carbon fiber as the core layer. The bending creep curves for all specimens showed a shape to increase at the upper right side, and the curves were found to show a linear behavior beyond about 1 h. The initial compliances of cork composite wood floorings increased in the order of merbau (M) < teak (T) = larch (La) < tulip tree (Tu), which showed a density dependence where higher density species that had lower deformation. The creep compliance increased in the order of tulip tree < merbau < teak < larch, but the values of this increase remained small. Regarding the dissimilar materials, the creep compliance tended to increase in the order of CM (cork-metal) < CC (cork-carbon fiber) < CG (cork-glass fiber). From these results, the bending creep compliance of the cork composite wood flooring with temperate wood species was higher than for those with high-density tropical wood species, but the gap between those species was small. These results indicate the potential of temperate wood species for various interior applications.



Full Article

Bending Creep Performance of Wood Flooring Composited with Cork Composite Boards Reinforced with Metal, Glass Fiber, and Carbon Fiber Using Temperate and Tropical Wood Species

Jun Ho Goh ,a Ju Won Seo ,a Hui Sun Park ,a and Han Min Park a,b,*

This study investigated the bending creep performance of cork composite wood floorings. The cork composite wood floorings consisted of two temperate species (tulip tree and larch) and two tropical species (teak and merbau) as the face layer, and a cork board reinforced with metal, glass fiber, or carbon fiber as the core layer. The bending creep curves for all specimens showed a shape to increase at the upper right side, and the curves were found to show a linear behavior beyond about 1 h. The initial compliances of cork composite wood floorings increased in the order of merbau (M) < teak (T) = larch (La) < tulip tree (Tu), which showed a density dependence where higher density species that had lower deformation. The creep compliance increased in the order of tulip tree < merbau < teak < larch, but the values of this increase remained small. Regarding the dissimilar materials, the creep compliance tended to increase in the order of CM (cork-metal) < CC (cork-carbon fiber) < CG (cork-glass fiber). From these results, the bending creep compliance of the cork composite wood flooring with temperate wood species was higher than for those with high-density tropical wood species, but the gap between those species was small. These results indicate the potential of temperate wood species for various interior applications.

DOI: 10.15376/biores.21.4.11367-11379

Keywords: Wood floorings; Cork composite board; Metal; Glass fiber; Carbon fiber; Bending creep performance

Contact information: a: College of Agriculture & Life Science, Gyeongsang National University, Jinju, 52828, Korea; b: Institute of Agriculture and Life Science, Gyeongsang National University, Jinju, 52828, Korea; *Corresponding author: [email protected]

INTRODUCTION

As interest in environmental issues has grown recently, awareness of sustainable architectural design has spread. The relationship between occupants’ health and building materials has also been emphasized (Nyrud and Bringslimark 2009). Accordingly, the impact of building materials on occupants’ psychological well-being is becoming increasingly important (Klepeis et al. 2001). Therefore, as demand grows for high-quality and eco-friendly materials to improve living environments, interest in wood-based interior materials is on the rise (Mergel et al. 2024).

Wood is a sustainable biomaterial that has a high strength-to-weight ratio and excellent seismic performance; through its carbon-storing capacity, it helps reduce a building’s energy consumption and improve its overall environmental impact (Wimmers 2017; Dukarska and Radosław 2023). However, structural components used in load-bearing areas of buildings, such as beams and flooring, are continuously exposed to various types of loads (Chen and Lin 1997; Passard and Perré 2005; Moosavi et al. 2016; Nilsson and Johansson 2017).

Also, wood and wood-based composites are viscoelastic materials that exhibit both elastic behavior and viscous flow. When a constant load acts continuously on such a material over a long period, the deformation that keeps increasing with time following the initial elastic deflection is defined as creep. Interior wood flooring is exposed to the compound action of concentrated loads from heavy furniture and repeated pedestrian loads (Fang et al. 2012). Under such long-term loading, wood-based flooring deflects progressively with time, and part of this deflection is not recovered after the load is removed but remains as permanent deformation (Schniewind 1968; Holzer et al. 1989). The deflection of a material under sustained load is expressed by the creep compliance, defined as the strain developed per unit applied stress (Schniewind 1968). A larger creep compliance means that, under the same stress, the floor materials deflect more as time elapses; the duration-of-load behavior and the creep behavior of the floor materials are essential to ensuring the stability of the whole structure (Yin et al. 2024).

Therefore, to overcome the physical limitations of a single type of wood and enhance structural loading capacity, research on composite materials has been continually conducted to maximize mechanical properties by combining wood species with different characteristics or dissimilar materials (Park et al. 2006; Jang et al. 2009; Moosavi et al. 2016; Cho et al. 2016; Nilsson and Johansson 2017; Park et al. 2020; Choi et al. 2021; Cha et al. 2022, 2024; Goh et al. 2025a,b). Among the materials used for composites with wood, cork is a biodegradable biomaterial similar to wood, and its honeycomb-like cellular structure provides superior impact absorption and energy dissipation capabilities (Gibson et al. 1981; Pereira 2007; Sergi et al. 2022).

Cork exhibits both elastic recovery and viscous damping. The elastic recovery restores a substantial portion of deformation upon load removal through its closed honeycomb cellular structure. The structure also can enhance viscous damping capacity, which originates from internal friction among cell-wall polymers (Gibson et al. 1981; Gil 2009). From these characteristics, cork can enhance the vibration damping performance of wood-based structures because it effectively reduces external mechanical energy through internal molecular friction (Mano 2002). Consequently, cork has been widely utilized as a core material and cushion layer to reduce floor impact sound transmission in building assemblies (Gil 2009; Ding et al. 2021). However, there have been few studies on the creep behavior of composite boards made by laminating wood, wood-based materials, and cork.

Therefore, in this study, in addition to the research on the bending strength performance of cork composite wood floorings (Goh et al. 2025a), cork composite wood floorings were manufactured to evaluate the bending creep performance. Two temperate wood species and two tropical hardwood species were utilized as the surface layers, and cork boards reinforced with dissimilar materials were used as the core layers. Subsequently, a bending creep test was conducted so that the effects of the surface wood species and the core dissimilar materials could be investigated.

EXPERIMENTAL

Specimens

The materials used for face layer were four wood species, and of these, teak (Tectona grandis) and merbau (Intsia bijuga), tropical wood species and tulip tree (Liriodendron tulipifera) and larch (Larix kaempferi), temperate wood species were selected. The dimensions of individual lamina were 400 mm in the radial direction, 60 mm in the tangential direction, and 1,000 mm in the longitudinal direction. They were cut into sizes of 50 (W) × 4 (T) × 360 (L) mm. A total of 60 laminae were manufactured, with 15 for each tree species.

As the core layer materials, cork composite boards reinforced with metal, glass fiber, and carbon fiber were used. The cork board, composed of 0.5 mm cork granule and bonded with pMDI (polymeric methylene diphenyl diisocyanate) was purchased in a roll measuring 1000 (W) × 2 (T) mm from Korea Cork Co., Ltd. and cut to a size of 50 (W) × 360 (L) mm.

As the bottom layer materials, the five-ply plywood made from Lauan (Pentacme contorta Merr. & Rolfe) was selected with a thickness of 4 mm (T) and was cut to 50 (W) × 360 (L) mm.

The cork-composite wood floorings were laminated using plywood, a cork board, a reinforcement material, another cork board, and wood in sequence from the bottom layer. The adhesive used was a water-based polymer-isocyanate adhesive (MPU-500, Okong Co., Ltd., Korea). The adhesive was evenly spread on both sides of each solid wood, cork board, reinforcing material, and plywood using a roller at a spread amount of 300 g/m2. The wood floorings were pressed at 0.6 MPa for 24 h at room temperature using a torque wrench and then cured for 7 days in a constant temperature and humidity room maintained at 20 °C and 65% relative humidity (RH). Figure 1 shows the arrangement of main composition materials of cork composite wood floorings, visualizing the laminated structures and reinforcements.

Schematic illustration of cork composite wood flooring specimens for bending creep test

Fig. 1. Schematic illustration of cork composite wood flooring specimens for bending creep test

Test specimens were named according to the species as the face, with teak, merbau, tulip wood, and larch abbreviated as T, M, Tu, and La, respectively. For the core layer, cork board, metal, glass fiber, and carbon fiber were abbreviated as C, M, G, and C, respectively. The samples were named T-CM, T-CG, T-CC, M-CM, M-CG, M-CC, Tu-CM, Tu-CG, Tu-CC, La-CM, La-CG, and La-CC, depending on their respective combinations. Three test specimens of each type of cork-composite wood flooring were prepared.

Bending Creep Test

The bending creep test for cork-composite wood flooring specimens was conducted by four-point loading. The span was 300 mm, and the distance between a loading point and a supporting point was 100 mm. The stress corresponding to 25% of the breaking stress obtained from a static bending test was applied to each specimen and the test was conducted in a constant-temperature and humidity room at 20 ℃ and 65% RH. The applied stresses are shown in Table 1.

Table 1. Applied Stress for Bending Creep Test of Wood Floorings Composited with Cork Boards and Three Kinds of Dissimilar Materials

Applied Stress for Bending Creep Test of Wood Floorings Composited with Cork Boards and Three Kinds of Dissimilar Materials

The creep deflections were measured at 0.5, 1, 3, 5, and 10 min up to 30 min after the initial deflection, followed by measurements every 30 min up to 2 h, and then every 1, 2, and 3 h up to 10 h. Subsequently, the creep deflections were measured every 12 h for the next 2 days, and every 24 h for the remaining period, which achieved a total measurement duration of 7 days (168 h). The number of specimens for the static bending test was set to 10, and the applied load was calculated as the average of the 10 specimens. The deflection of the mid-span was measured with a dial gauge. The total creep compliance (D(t)) was calculated using Eq. 1, and the creep compliance (Dc(t)) was determined using Eq. 2 from the deflection at each time point,

(1)

where ε (t) is deflection at time t; σ is the stress; P is the applied load; l is the span; b and h are the width and depth of the beam; 11 is the distance between a loading point and a supporting point; and y(t) is the apparent deflection at time (t) between both the two supporting points; D(t) is the apparent total creep compliance obtained from the apparent deflection. Equation 2 is given below,

(2)

where D(0.008) is the total creep compliance at t = 0.008h(30s) and called initial compliance.

Schematic diagram of bending creep test for cork-composite wood floorings

Fig. 2. Schematic diagram of bending creep test for cork-composite wood floorings

RESULTS AND DISCUSSION

Bending Creep Curves of Cork-composite Wood Floorings

Figure 3 shows typical examples of the bending creep curves of the cork-composite wood floorings, according to the type of surface wood species and dissimilar materials in the middle layer.

All cork-composite wood floorings showed a form of exponential function curves where the deflection continuously increased over time, regardless of wood species and the type of dissimilar materials. The increment in bending creep compliance was significant in larch (La) among the temperate wood species and in teak (T) among the tropical wood species, whereas tulip tree (Tu) and merbau (M) exhibited moderate slopes in their creep curves. The creep deflection at the beginning of the test did not show substantial variation among the different types. However, the slopes of the creep curves for the specimens gradually increased over time.

Figure 4 shows the bending creep behavior over time for each type was compared by plotting the bending creep compliance of the cork-composite wood floorings and time on a logarithmic plot. The creep curves of the cork-composite wood floorings were expressed by the following equation (power law) (Kitahara and Perng 1965; Nakai 1978; Arima et al. 1981; Aratake and Arima 1995),

(3)

where A is the creep compliance reached at one hour and represents the magnitude of the time-dependent deformation; N is the slope of the creep curve on a double-logarithmic plot; t is time.

Creep curves of cork composite wood floorings and double logarithm plots of creep deformation and time for typical examples of cork composite wood floorings

Regardless of all wood species of the face layer and the types of dissimilar materials of the core layer, the bending creep behavior over time for the cork-composite wood floorings showed a curvilinear behavior from the initial deformation up to 30 min to 1 h. However, the bending creep behavior showed nearly linear behavior until 168 h. Both sides of Eq. 3 were log-transformed to determine the values of the slope N and the intercept A, and their average values are shown in Table 2. The correlation coefficient between time (t) and creep strain (Dc(t)) ranged from 0.968 to 0.997, which indicated a very high correlation.

According to the surface wood species, the N values of the wood floorings with the teak (T) surface layer showed the highest range of N = 0.263 to 0.291, whereas those with the merbau (M) surface layer showed the lowest range of N = 0.230 to 0.261. According to the wood species, the average N values ranged from 0.246 to 0.279, where larch (La) showed the lowest value of 0.246 and teak (T) showed the highest value of 0.279. The values followed the order of teak (T) > merbau (M) = tulip tree (Tu) > larch (La).

Among the dissimilar materials of the core, the CM type showed the lowest average N value of 0.245, while the CG type showed the highest N value of 0.267. However, the range of N values was narrow, with values ranging from 0.245 to 0.267, which showed a slight difference.

The N values of cork-composite wood floorings, which ranged from 0.230 to 0.283, were slightly higher than the range of 0.224 to 0.269 for wood-based boards (MDF, PB, and OSB) reported by Park et al. (2010) but were lower than the three-ply hybrid laminated woods composed of spruce and wood-based boards, which ranged from 0.235 to 0.402.

The A values of the cork-composite wood floorings increased in proportion to the creep deflection. Among the four wood species, the tulip tree (Tu) type showed the lowest value, followed by merbau (M), larch (La), and teak (T). According to the core dissimilar material types, the values increased in the order of CG < CC < CM.

According to the two-way ANOVA results of N values, the contributions (partial η2) of the wood species, core reinforcement, and their composite effect were 0.230, 0.130, and 0.160, respectively. The factors of wood species (F = 2.39, p = 0.094), core reinforcement (F = 1.79, p = 0.188), and composite effect (F = 0.76, p = 0.608) showed no statistical significance at the significance level of α = 0.05 (p > 0.05). These results indicate that both wood species and core reinforcement had no significant effect on the creep rate exponent, .

Table 2. Results of Bending Creep Test of Wood Floorings Composited with Cork Boards and Three Kinds of Dissimilar Materials

Results of Bending Creep Test of Wood Floorings Composited with Cork Boards and Three Kinds of Dissimilar Materials

For the creep constant, A, the contribution of wood species was the highest at 0.447, while the contributions of core reinforcement and the composite effect were 0.173 and 0.332, respectively. The wood species factor showed statistical significance within the level of p < 0.01(F = 6.48, p = 0.002). In contrast, both the core reinforcement (F = 2.51, p = 0.102) and the composite effect (F = 1.99, p = 0.107) showed no significance at α = 0.05 (p > 0.05). These results suggest that the reinforcement type did not show a significant difference in the magnitude of initial deformation, whereas the surface wood species caused a significant effect.

Initial Deformation and Creep Deformation of Cork-composite Wood Floorings

The results of the bending creep test for the cork-composite wood floorings are shown in Table 2, and the initial and creep deformations of the floorings are shown in Fig. 5.

Regarding the initial deformation of the cork-composite wood floorings according to the wood species of the face layer, the tulip tree (Tu) type showed the highest value of 16.6 × 10-11Pa-1. However, the merbau (M) type showed the lowest value of 12.8 × 10-11Pa-1. The values were in the order of tulip tree (Tu) > larch (La) > teak (T) > merbau (M). It was confirmed that the initial deformation decreased as the wood species density increased, which showed density-dependent behavior. Regarding the creep deformation of the cork-composite wood floorings, the larch (La) type showed the highest value of 4.74 × 10-11Pa-1, whereas the tulip tree (Tu) type showed the lowest value of 3.13 × 10-11Pa-1. However, the density dependence of creep deformation was not as clear as that of initial deformation.

The initial deformation of the cork-composite wood floorings according to the dissimilar materials of the core layer averaged from 14.3 to 15.7 × 10-11Pa-1, and the values were in the order of CG type < CC type < CM type. Moreover, the creep deformation of the cork-composite wood floorings according to the dissimilar materials of the core layer averaged from 3.50 to 4.17 × 10-11Pa-1, and the values were in the order of CG type < CC type < CM type.

The initial deformation is an elastic response influenced by the modulus of elasticity of the cork-composite wood floorings. Because the modulus of elasticity of wood increases with higher density due to a larger quantity of load-bearing cell-wall substance, the initial deformation decreased as the density increased. In contrast, the creep deformation is a viscoelastic response that primarily originates from the time-dependent deformation of the amorphous matrix within the cell walls, as well as from the deformation of the low-modulus cork core and adhesive layers in this sandwich structure. Within these specific layers, shear deformation increases irregularly under sustained load (Park and Fushitani 2007).

The creep deformation values of the cork-composite wood floorings were 3.2 to 3.3 times higher than those of the three-layer laminated woods parallel to the grain made from royal paulownia, Japanese cedar, Japanese cypress, katsura, and beech wood. The values were 1.0 to 1.8 times higher than those of the three-layer parallel laminated woods parallel to the grain of the face layer (Park et al. 2006). Additionally, these values were 1.8 to 3.2 times higher than those of the wood and wood-based hybrid boards (Park et al. 2010); moreover, the values were 3.2 to 3.6 times higher than those of the wood-concrete hybrid laminated materials (Cho et al. 2016).

For the initial elastic deflection, D (0.008), the two-way ANOVA results showed high contributions (partial η2) of 0.808, 0.377, and 0.845 for wood species, core reinforcement, and their composite effect, respectively. The face-layer wood species (F = 33.73, p < 0.001) and the composite effect (F = 21.80, p < 0.001) showed high statistical significance at the significance level of p < 0.001, and core reinforcement (F = 7.26, p = 0.003) showed high statistical significance at the significance level of p < 0.01. In particular, the contribution of the composite effect factor was the highest at 0.845. These results indicate that resistance to initial deflection depends heavily on the composite effect of wood species and core reinforcement, rather than on the individual effects of the separate materials.

In the two-way ANOVA results for Dc(168), all three factors showed statistical significance. The contributions of wood species, core reinforcement, and their composite effect were 0.693, 0.260, and 0.600, respectively. Wood species (F = 18.04, p < 0.001) and the composite effect (F = 5.99, p < 0.001) showed high significance at p < 0.001, and core reinforcement (F = 4.22, p = 0.027) also showed significance at p < 0.05. These results indicate that not only the main effects of wood species and core reinforcement, but also the composite effect between the two layers had significant effects on long-term deflection reduction performance.

Initial and creep compliances of cork composite wood floorings

Relative Creep of Cork-Composite Wood Floorings

Table 2 shows the relative creep of cork-composite wood floorings which was defined as the percentage of creep deformation at 168 h to initial deformation, and Fig. 6 shows the relative creep for each type of dissimilar materials of the core layer.

The relative creep of cork-composite wood floorings showed that the teak face layer with CM core layer type was the highest value of 33.4% and the tulip tree face layer with CM type of the core layer was the lowest value of 16.4%. According to the wood species of the face layer, the relative creep ranged from 19.1% to 32.2%, the tulip tree (Tu) showed the lowest value of 19.1%, and the larch (La) showed the highest value of 32.2%. The values were in the order of tulip tree (19.1%) < merbau (25.0%) < teak (28.3%) < larch (29.5%).

According to the dissimilar materials of the core layer, the relative creep ranged from an average of 24.5% to 29.4%, and the values were in the order of CG < CC < CM .

The average relative creep of cork-composite wood floorings ranged from 16.4% to 29.5%. These values were 2.1 to 2.5 times higher than the relative creep values of the three-layer parallel laminated woods parallel to the grain made from paulownia, cedar, cypress, katsura, and beech. The values were 1.0 to 1.4 times higher than those of the three-layer parallel laminated woods parallel to the grain of the face layer (Park et al. 2006). Additionally, these values were 1.1 to 1.7 times higher than those of the wood and wood-based hybrid boards (Park et al. 2010). Moreover, the values were approximately 1.7 to 2.0 times higher than those of the wood-concrete hybrid laminated materials (Cho et al. 2016).

According to the two-way ANOVA results for relative creep, Rc, the contributions were 0.682 for wood species, 0.444 for the composite effect, and 0.141 for core reinforcement. The wood species factor (F = 17.14, p < 0.001) showed statistical significance at p < 0.001, and the composite effect factor (F = 3.20, p = 0.019) showed statistical significance at p < 0.05. In contrast, core reinforcement as an individual factor (F = 1.97, p = 0.162) showed no significance at the significance level of α = 0.05 (p > 0.05). These results indicate that the core reinforcement did not show an identical difference across all wood species but instead showed a significant composite effect to improve resistance to relative creep when composited with specific wood species.

Relative creep of cork-composite wood floorings at 168 h; Each value is the average of three measurements

CONCLUSIONS

In this study, cork-composite wood floorings were manufactured using two temperate wood species and two tropical wood species as the face layer, and cork boards reinforced with metal, glass fiber, and carbon fiber as the core layer. Bending creep tests were conducted on these boards to investigate the effects of the wood species of the face layer and the type of dissimilar materials of the core layer on bending creep properties.

  1. The creep curves of the cork-composite wood floorings showed exponential functional graphs with the deflection increased toward the upper right over time, regardless of the wood species and dissimilar material types. In addition, the creep deflection over time showed curvilinear behavior for 1 h after loading, but it thereafter showed almost linear behavior. Therefore, it was confirmed that the creep deflection could be predicted when the experimental data were applied to the power law.
  2. The initial deformation of the cork-composite wood floorings increased in the order of merbau (M) < teak (T) < larch (La) < tulip tree (Tu) according to the face layer wood species. The values were confirmed that the higher-density wood species showed a lower density dependence.
  3. The creep deformation of the cork-composite wood floorings increased in the order of tulip tree (Tu) < merbau (M) < teak (T) < larch (La) according to the surface wood species. However, the density-dependence of the face layer wood species was not confirmed in the creep deformation.
  4. The relative creep of the cork-composite wood floorings ranged from 16.4% to 29.5%. According to the face layer wood species, the values were in the order of tulip tree (Tu) < merbau (M) < teak (T) < larch (La).
  5. The two-way ANOVA results showed that the bending creep performance of cork-composite wood floorings depended on the combination of the face wood species and core reinforcement, rather than on the face wood species or core reinforcement as an individual factor. Wood species were generally the dominant contributor to initial deformation and creep deformation. The composite effect between the face wood species and core reinforcement showed statistical significance for both initial deformation and creep deformation. Consequently, these results indicate that the combination of wood species density and core reinforcement is essential for cork-composite wood floorings; among the tested combinations, the tulip tree face layer with a metal-reinforced cork core (Tu-CM) showed the best creep performance.

ACKNOWLEDGMENTS

This study was carried out with the support of ‘R&D Program for Forest Science Technology (Project No. RS-2024-00404631613)’ Provided by the Korea Forest Service (the Korea Forestry Promotion Institute).

REFERENCES CITED

Aratake, S., and Arima, T. (1995). “Creep of sugi sawn lumber in process of humidity changes (in Japanese),” Mokuzai Gakkaishi 41, 359-366.

Arima, T., Sato, M., and Mashita, K. (1981). “Studies on evaluation method for long-term performance of wood-based materials and elements (in Japanese),” Architectural Research Report 95, 25-80.

Cha, M. S., Goh, J. H., Kim, D. H., Goh, S. H., and Park, H. M. (2024). “The physical properties of cross-laminated wood panels made with tropical hardwoods and domestic temperate woods,” The Journal of Agricultural & Life Science 58(4), 101-107. https://doi.org/10.14397/jals.2024.58.4.101

Cha, M. S., Yoon, S. J., Kwon, J. H., Byeon, H. S. and Park, H. M. (2022). “Mechanical properties of cork composite boards reinforced with metal, glass fiber, and carbon fiber,” Journal of the Korean Wood Science and Technology 50(6), 427-435. https://doi.org/10.5658/WOOD.2022.50.6.427

Chen, T. Y., and Lin, J. S. (1997). “Creep behaviour of commercial wood based boards under long-term loading at room conditions in Taiwan,” Holz als Roh-und Werkstoff 55(6), 371-376. https://doi.org/10.1007/s001070050249

Cho, Y. J., Byeon, J. W., Lee, J. R., Sung, E. J., and Park, H. M. (2016). “Bending creep performance of domestic wood-concrete hybrid laminated materials,” Journal of Korean Wood Science Technology 44(1), 57-66. https://doi.org/10.5658/WOOD.2016.44.1.57

Choi, G. W., Yang, S. M., Lee, H. J., Kim, J. H., Choi, K. H., and Kang, S.G. (2021). “Evaluation of flexural performance according to the plywood bonding method of ply-lam CLT,” Journal of the Korean Wood Science and Technology 49(2), 107-121. https://doi.org/10.5658/WOOD.2021.49.2.107

Dukarska, D, and Radosław M. (2023). “Wood-based materials in building,” Materials 16(8), article 2987. https://doi.org/10.3390/ma16082987

Fang, C. H., Blanchet, P., Cloutier, A., and Barbuta, C. (2012). “Engineered wood flooring with a densified surface layer for heavy-duty use,” BioResources 7(4), 5843-5854. https://doi.org/10.15376/biores.7.4.5843-5854

Gibson, L. J., Easterling, K. E., and Ashby, M. F. (1981). “The structure and mechanics of cork,” Proceedings of the Royal Society of London A: Mathematical and Physical Sciences 377(1769), 99-117. https://doi.org/10.1098/rspa.1981.0117

Goh, J. H., Goh, S. H., Kim, D. H., Cha, M. S., and Park, H. M. (2025a). “Bending performance of sandwich flooring with wood exterior and two-layer cork interior reinforced separately with metal, glass fiber, or carbon fiber,” BioResources 20(4). https://doi.org/10.15376/biores.20.4.9667-9677

Goh, S. H., Goh, J. H., Kim, D. H., Cha, M. S., and Park, H. M. (2025b). “Dimensional stability of solid wood flooring combined with cork board reinforced by metal, glass fiber, and carbon fiber,” Journal of Agriculture & Life Science 59(4), 111–116. https://doi.org/10.14397/jals.2025.59.4.111

Holzer, M., Loferski, J. R., and Dillard D. A. (1989). “A review of creep in wood: concepts relevant to develop long-term behavior predictions for wood structures,” Wood and Fiber Science 1989, 376-392.

Jang, S. S., Kim, Y. H., and Jang, Y. I. (2009). “Mechanical properties of composite materials composed of structural steel and structural glued laminated timber,” Korean Society of Wood Science and Technology 37(4), 300-309.

Kitahara, K., and Perng, W. T. (1965). “On the creep of hardboard (in Japanese),” Mokuzai Gakkaishi 11, 88–92.

Klepeis, N. E., Nelson, W. C., Ott, W. R., Robinson, J. P., Tsang, A. M., Switzer, P., Behar, J. V., Hern, S. C., and Engelmann, W. H. (2001). “The national human activity pattern survey (NHAPS): A resource for assessing exposure to environmental pollutants,” Journal of Exposure Science & Environmental Epidemiology 11(3), 231-252. https://doi.org/10.1038/sj.jea.7500165

Mano, J. F. (2002). “The viscoelastic properties of cork,” Journal of Materials Science 37(2), 257-263. https://doi.org/10.1023/A:1013635809035

Mergel, C., Menrad, K., and Decker, T. (2024). “Which factors influence consumers’ selection of wood as a building material for houses?,” Canadian Journal of Forest Research 54(4), 467-478. https://doi.org/10.1139/cjfr-2023-0197

Moosavi, V., Eslam, K. H., Bazyar, B., Najafi, A., and Talaeepoor, M. (2016). “Bending creep behavior of Hornbeam wood,” Drvna Industrija 67(4), 341-350. https://doi.org/10.5552/drind.2016.1609

Nakai, T. (1978). “Bending creep test on wood-based boards I (in Japanese),” Wood Industry Japanese 33(4), 158-160.

Nilsson, J., and Johansson. J., (2019). “Bending and creep deformation of a wood-based lightweight panel: An experimental study,” Wood and Fiber Science 51(1) 16-25. https://doi.org/10.22382/wfs-2019-003

Nyrud, A. Q., and Bringslimark., T. (2010). “Is interior wood use psychologically beneficial? A review of psychological responses toward wood,” Wood and Fiber Science 2, 202-218.

Park, H. M., Fushitani, M., Sato, K., Kubo, T., and Byeon, H. S. (2006). “Bending creep performances of three-ply cross-laminated woods made with five species,” Journal of Wood Science 52(3), 220-229. https://doi.org/10.1007/s10086-005-0750-7

Park, H. M., Gong, D. M., Shin, M. G., and Byeon, H. S. (2020). “Bending creep properties of cross-laminated wood panels made with tropical hardwood and domestic temperate wood,” Journal of the Korean Wood Science and Technology 48(5), 608-617. https://doi.org/10.5658/WOOD.2020.48.5.608

Park, H. M., Kang, D. H., Choi, Y. E., Ahn, S. Y., Ryu, H. S., and Byeon, H. S. (2010). “Bending creep performances of hybrid laminated woods composed of wood-wood based boards,” Journal of Korean Wood Science Technology 38(1), 1-10. https://doi.org/10.5658/WOOD.2010.38.1.1

Passard, J., and Perré, P. (2005). “Viscoelastic behaviour of green wood across the grain. Part I. Thermally activated creep tests up to 120 C,” Annals of Forest Science 62(7), 707-716. https://doi.org/10.1051/forest:2005067

Pereira, H. (2007). Cork: Biology, Production and Uses, Elsevier, Amsterdam, Netherlands.

Sergi, C., Sarasini, F., and Tirillò, J. (2021). “The compressive behavior and crashworthiness of cork: A review,” Polymers 14(1), article 134. https://doi.org/10.3390/polym14010134

Schniewind, A. P. and Ricmond, C. (1968). “Recent progress in the study of the rheology of wood,” Wood Science and Technology 2, 188-206. https://doi.org/10.1061/JSENDH.STENG-14850

Wimmers, G. (2017). “Wood: A construction material for tall buildings,” Nature Reviews Materials 2, article 17051. https://doi.org/10.1038/natrevmats.2017.51

Yin, T., Song, H., Wang, Z., Li, L., Zheng, W., Ju, Z., Gong, Y., and Gong, M. (2024). “Long-term creep properties of hybrid CLT fabricated with lumber and OSB,” Industrial Crops and Products 211, article 118238. https://doi.org/10.1016/j.indcrop.2024.118238

Article submitted: June 1, 2026; Peer review completed: August 15, 2026; Revised version received: September 16, 2026; Accepted: September 20, 2026; Published: October 7, 2026.

DOI: 10.15376/biores.21.4.11367-11379