Abstract
Physical and mechanical properties of commercial E1 and E2 grade particleboards produced by different manufacturers in Turkey were compared, and the relationships among these properties were examined. A total of 14 particleboard samples with a thickness of 18 mm, obtained from the domestic market, were evaluated. The moisture content (MC), density, formaldehyde emission, modulus of rupture (MOR), modulus of elasticity (MOE), and internal bond strength (IB) of the panels were determined; the data were analyzed using one-way analysis of variance, Duncan’s test, the independent samples t-test, and Pearson’s correlation analysis. The results showed that there were no significant differences between E1 and E2 panels in terms of MC and MOR (p > 0.05); however, there were significant differences in terms of density, formaldehyde emission, MOE, and IB (p < 0.05). The average formaldehyde emission was determined to be 4.84 mgF/100 g of dry panel for E1 panels and 10.73 mgF/100 g of dry panel for E2 panels. All panels met the minimum performance criteria for Class P2 as specified in the TS EN 312 (2012) standard, and the study revealed that performance differences among commercial particleboard products may exist, depending on the manufacturer and emission class.
Download PDF
Full Article
Comparative Evaluation of the Physical, Mechanical, and Formaldehyde Emission Properties of Commercial E1 and E2 Particleboard Manufactured in Turkey
Physical and mechanical properties of commercial E1 and E2 grade particleboards produced by different manufacturers in Turkey were compared, and the relationships among these properties were examined. A total of 14 particleboard samples with a thickness of 18 mm, obtained from the domestic market, were evaluated. The moisture content (MC), density, formaldehyde emission, modulus of rupture (MOR), modulus of elasticity (MOE), and internal bond strength (IB) of the panels were determined; the data were analyzed using one-way analysis of variance, Duncan’s test, the independent samples t-test, and Pearson’s correlation analysis. The results showed that there were no significant differences between E1 and E2 panels in terms of MC and MOR (p > 0.05); however, there were significant differences in terms of density, formaldehyde emission, MOE, and IB (p < 0.05). The average formaldehyde emission was determined to be 4.84 mgF/100 g of dry panel for E1 panels and 10.73 mgF/100 g of dry panel for E2 panels. All panels met the minimum performance criteria for Class P2 as specified in the TS EN 312 (2012) standard, and the study revealed that performance differences among commercial particleboard products may exist, depending on the manufacturer and emission class.
DOI: 10.15376/biores.21.4.11993-12010
Keywords: Commercial particleboard; Formaldehyde emission; Mechanical performance; Physical properties; Pearson correlation
Contact information: Department of Wood Mechanics and Technology, Faculty of Forestry, Düzce University, 81620, Düzce, Turkey; *Corresponding author: [email protected]
INTRODUCTION
Today, there are various types and designs of particleboard available to support the many construction and furniture applications required by modern life. They are widely used in interior applications, such as surface finishes, flooring, cabinets, and furniture, as well as in many other load-bearing applications. Compared to other types of wood, particleboard is a wood-based composite that is cost-effective, easy to process, and compatible with surface finishing materials. Additionally, panels capable of meeting the specific requirements of building applications, such as moisture resistance, fire retardancy, acoustic insulation, and thermal insulation, are commercially produced. Plywood panels can also be finished with a variety of surface materials, such as wood veneer and laminate (Papadopoulou and Chrissafis 2017; Janiszewska-Latterini and Pizzi 2023).
Globally, demand for and production of particleboard have steadily increased in recent years. One of the main reasons for the growing demand for these products is their increasing use in furniture and interior design applications. According to the International Market Analysis Research and Consulting Group (IMARC), the global particleboard market reached a total of $24.6 billion in 2025. The IMARC Group projects that, with an annual growth rate of 2.98%, this market size will reach $32.2 billion by the end of 2034. In this context, determining the performance characteristics of commercially produced chipboards and their compliance with relevant standards becomes increasingly important (IMARC Group 2026).
According to data from the Food and Agriculture Organization of the United Nations (FAO), global particleboard production in 2022 was 110.25 million m³, while in Europe it stood at 44.82 million m³. In the same year, particleboard production in Turkey was 5.63 million m³ (Fig. 1). Considering the 2022 production figures, Turkey ranked third globally and second in Europe among particleboard-producing countries (FAO 2025). This significant production capacity makes it important to evaluate the performance of commercial particleboard produced in Turkey using current data.
Fig. 1. The top 10 countries with the highest particleboard production in 2022 (FAO 2025)
Formaldehyde-based resins are the most commonly used adhesives in the production of wood-based panels. Among these adhesives, urea-formaldehyde resin is the most widely used in particleboard production due to its high reactivity, ease of application, rapid curing, ability to impart high mechanical strength to the board under dry conditions, and low cost. However, formaldehyde emissions and low water resistance are the most significant disadvantages of this adhesive. Recently, the production of panels with low formaldehyde emissions has become an important research topic for researchers (Ryu et al. 2019; Ghani et al. 2022; Gumus et al. 2024; Younesi-Kordkheili 2024).
Formaldehyde is a colorless chemical with a sharp, unpleasant odor that is widely used in the production of wood-based panels and is harmful to human health and the environment (Ryu et al. 2019; Kord et al. 2022). The amount of formaldehyde released from wood-based panels is influenced by many factors, such as the resin system, production conditions, panel density, and the environment in which the panel is used. In many countries, wood-based panels with low formaldehyde emissions are preferred, and relevant legal regulations are continually being updated (Kord et al. 2022). For this reason, it is important to evaluate not only the formaldehyde emissions but also the physical and mechanical properties of commercially produced E1 and E2 grade particleboards.
In recent years, the effects of various resin systems, formaldehyde binders, and bio-based adhesives on the physical, mechanical, and emission properties of particleboard have been extensively studied to reduce formaldehyde emissions (Kord et al. 2022; Kristak et al. 2023; Calvez et al. 2024; Mirindi 2024). The results indicate that formaldehyde emissions can be significantly reduced by using appropriate resin systems and additional additives. However, depending on the resin system and additives used, the physical and mechanical properties of the panels may change to varying degrees.
Research conducted in recent years has focused on reducing formaldehyde emission levels in particleboard through the development of different resin systems, alternative additives, and bio-based adhesives (Baharuddin et al. 2023; Janiszewska-Latterini and Pizzi 2023; Ma et al. 2023). These studies demonstrate that formaldehyde emissions can be significantly reduced by using appropriate resin and adhesive systems. However, it is not immediately apparent from standard compliance data to what extent commercial particleboard products that meet the performance limits defined in the standards vary in terms of their physical, mechanical, and formaldehyde emission properties across different manufacturers and emission classes. In particular, comparing commercial E1- and E2-class particleboards of the same thickness under identical experimental conditions could enable the quantitative identification of performance differences among manufacturers and variations associated with emission classes. Therefore, rather than simply re-establishing the well-known relationships between production parameters and product properties found in the existing literature, a comparative evaluation of the performance variability of actual commercial products could provide a complementary data source regarding the performance of current products.
However, the fact that commercial particleboard meets the performance requirements defined in the relevant standards does not mean that boards produced by different manufacturers have the same physical, mechanical, and emission performance. The standards define whether products meet specific performance requirements, but they do not provide direct information about performance variability among commercial products that fall within these limits. Therefore, comparing E1 and E2 class particleboards commercially produced by different manufacturers under the same experimental conditions may contribute to highlighting the variability in commercial product performance within the standard limits, rather than merely re-verifying compliance with the standards. Such a comparison makes it possible to identify performance differences among products within the same emission class and to determine property-based variations between the E1 and E2 classes.
In recent years, there has been an increase in studies examining the relationships between physical and mechanical properties of wood-based panels using statistical methods. In particular, correlation analyses contribute to identifying linear relationships between different properties (Camlibel 2023; Almeida et al. 2025). In this study, correlation analysis was used as a complementary analysis to support the evaluation of relationships among the properties of commercial E1 and E2 grade particleboards.
In this context, comparing performance differences between commercial E1 and E2 grade particleboards of the same thickness across different manufacturers and emission classes may help highlight the variability in commercial products. Furthermore, evaluating the relationships among physical and mechanical properties can provide complementary information to this comparison.
The aim of this study was to compare the physical, mechanical, and formaldehyde emission properties of 18 mm thick E1 and E2 class particleboards commercially produced by different manufacturers in Turkey. The study evaluated the differences between E1 and E2 class panels, performance variations among manufacturers, and linear relationships between physical and mechanical properties. In this context, the goal was to create a comparable dataset regarding the performance of E1 and E2 class particleboards commercially produced in Turkey and to establish this data as a reference for future studies.
The primary hypothesis of the study is that the physical, mechanical, and formaldehyde emission properties of commercial E1 and E2 class particleboards produced by different manufacturers in Turkey will vary across manufacturers and emission classes. The second hypothesis is that significant linear relationships will be found between board density and certain physical and mechanical properties.
EXPERIMENTAL
Materials
The particleboard panels used in the analyses conducted as part of this study were obtained from factories in Turkey that manufacture particleboard. For panel selection, 18-mm-thick particleboard panels produced with urea-formaldehyde adhesive and classified as E1 and E2, with an average density of 650 kg/m³ ± 10% (TS EN 312 (2012)), were chosen. The analyses conducted as part of this study were performed on 8 different commercial panel groups in the E1 emission class (E1-1 to E1-8) and 6 commercial panel groups in the E2 emission class (E2-1 to E2-6). This coding system is used in the tables that follow.
Methods
Preparation of test specimens
In conducting the experiments, commercial particleboard panels measuring 18 mm x 1830 mm x 3660 mm and classified as E1 and E2, which are manufactured for indoor applications (including furniture) in dry conditions, were used. To prepare the test specimens, samples were cut parallel and perpendicular to the panel’s production direction using a computer numerical controlled (CNC) machine (AES Raptor 2142 Flat, 2013, Turkey) (Fig. 2).
Fig. 2. Test specimens prepared on a CNC machine for physical and mechanical testing
The prepared test specimens were conditioned in a climate chamber at a temperature of 20 ± 2 °C and a relative humidity of 65 ± 5% in accordance with the relevant standard until they reached a constant weight (TS 642 ISO 554 1997). Subsequently, the formaldehyde emission values and the physical and mechanical properties of the panels were determined in accordance with the relevant standards.
Formaldehyde emission value
The extraction method, also known as the perforator method, was used to determine the free formaldehyde values of the panels (TS EN ISO 12460-5 2016). In accordance with the relevant standard, 110 g test specimens were prepared from panel pieces measuring 25 mm x 25 mm. These samples were placed in a flask containing 600 mL of toluene solution. For the extraction process, a condenser, a gas collection bottle, and a cold water apparatus were connected to each other, and the test samples were subjected to boiling for 2 h (Fig. 3).
Fig. 3. Sample preparation and testing procedure for formaldehyde analysis: a: weighing of test samples; b: preparation and mixing of the solution and test samples for the extraction process; c: extraction process
After the extraction process, the liquid in the percolator was cooled to room temperature and transferred to a graduated flask. Pure water from the gas absorption flask was also transferred into the volumetric flask to bring the volume up to 2000 mL. Using a pipette, 10 mL of the solution was withdrawn and transferred to a test tube. Ten milliliters of acetylacetone and 10 mL of ammonium acetate solution were added to the test tube, and the tube was sealed. The test tube was heated at 40 °C for 15 min. The absorbance of the resulting solution was measured at a wavelength of 412 nm against distilled water using a Spectroquant Pharo 300 UV/Vis spectrophotometer (Merck KGaA, Darmstadt, Germany; Fig. 4). A blank value was determined in parallel with distilled water. Three replicate measurements were performed for each test group to determine the formaldehyde emission values.
Fig. 4. Measurement of absorbance values in formaldehyde test samples using the perforator method: a: transfer of the test sample into the machine chamber; b: absorbance value read from the analysis results
Physical and mechanical properties of the commercial panels
Moisture content (MC) determination for commercial panels was performed in accordance with the TS EN 322 (1999) standard, while density values were determined in accordance with the TS EN 323 (1999) standard. Sheet samples measuring 50 mm x 50 mm x 18 mm were used for the physical properties. Twenty-four replicate measurements were performed to determine MC, and 36 replicate measurements were performed to determine density.
Fig. 5. Images of test specimens used in mechanical tests: a) conditioned specimens for MOR and MOE tests, b) measurement of the MOR and MOE, and c) images of test specimens prepared for IB testing and after fracture
The mechanical properties of the commercial panels, specifically the modulus of rupture (MOR) and modulus of elasticity (MOE), were determined in accordance with the TS EN 310 (1999) standard. In these analyses, the three-point bending test method was applied. The distance between supports was set to 20 times the panel thickness. A total of 36 test specimens, each measuring 410 mm x 50 mm x 18 mm, were prepared. A 20 kN computer-controlled universal testing machine manufactured by UTEST (UTEST Material Testing Equipment, Ankara, Turkey) was used in the tests. The load was applied exactly at the center of the support points, and fracture was achieved at 60 (± 30) s. The internal bond strength (IB) test was conducted on plate specimens measuring 50 mm x 50 mm x 18 mm in accordance with the TS EN 319 (1999) standard. A total of 48 test specimens were used for this test. Figure 5 shows images of the mechanical test specimens.
Statistical Analysis
The IBM SPSS Statistics 22 software package was used for the statistical analysis of the data. As part of this study, the formaldehyde emissions and the physical and mechanical properties of E1 and E2 grade commercial particleboard were statistically evaluated both within each class and in comparison to one another. One-way analysis of variance (One-way ANOVA) was used to determine differences among manufacturers, and Duncan’s multiple range test was applied to identify which groups accounted for the significant differences (p < 0.05). An independent samples t-test was used to compare the E1 and E2 emission classes. Additionally, Pearson correlation analysis was performed to determine linear relationships among the physical and mechanical properties, and the significance of the correlation coefficients was assessed at a 95% confidence level.
RESULTS AND DISCUSSION
Physical Properties
Table 1 presents the average MC, density, and formaldehyde emission values for E1 and E2 class particleboard. The MC values ranged from 6.60% to 9.57% for E1 class particleboard and from 7.26% to 9.53% for E2 class particleboard. Statistically significant differences in MC were observed among manufacturers for both board classes (ANOVA, p < 0.05).
The Duncan test results showed that when classes E1 and E2 were evaluated separately, the producers fell into different homogeneity groups in terms of MC, and that some producers were in the same homogeneity group. In contrast, according to the results of the independent samples t-test, no statistically significant difference was found between the MC content values of Class E1 and E2 particleboards (p > 0.05). All of the commercial particleboards examined fell within the 9% ± 4% limits specified in TS EN 312 (2012). This indicates that the MC of the commercial particleboards examined met the standard requirements.
The fact that the average MC values of all commercial particleboards discussed in this article fell within the range specified in the TS EN 312 (2012) standard suggests that the particleboards reached their equilibrium moisture content under appropriate production and storage conditions. The absence of a significant difference in MC between E1 and E2 class particleboards is an expected result. This is because formaldehyde emission classes are primarily related to the resin system and formaldehyde release. The MC is not a parameter that directly affects the equilibrium moisture content of particleboard. It has been noted that the MC of particleboards varies depending on the temperature and relative humidity of the storage environment, as well as production conditions (Baharoğlu et al. 2012; Thybring and Fredriksson 2023). Similarly, Camlibel (2023) noted that changes in production conditions for commercial particleboards can lead to limited variations in MC, while Dukarska et al. (2022) stated that raw material moisture is a significant factor affecting the production process and the quality characteristics of the boards. The study results show that the MC values for all panel groups remained within the limits specified by the relevant standard and that the commercial E1 and E2 class particleboards had similar MC values. This indicates that the panels under examination were at an appropriate moisture level in terms of their dimensional stability and performance under dry conditions.
Table 1. Moisture Content, Density, and Formaldehyde Emission Values for Commercial E1 and E2 Particleboards
Density values ranged from 629 to 686 kg/m³ for E1-class particleboards and from 624 to 691 kg/m³ for E2-class particleboards (Table 1). Statistically significant differences in density were observed among manufacturers in both board classes (p < 0.05). The results of the Duncan test showed that, when classes E1 and E2 were evaluated separately, the producers fell into different homogeneity groups based on their density values, and that some producers were in the same homogeneity group. Furthermore, the results of the independent samples t-test indicate a statistically significant difference between the average density values of E1 and E2 class particleboards (p < 0.05). This result demonstrates that density in commercial particleboard can vary depending on both the manufacturer and the emission class. However, it was observed that the density values of all commercially produced panels fell within the target density range specified in the TS EN 312 (2012) standard. Differences in density values indicate that manufacturer variations must be taken into account when evaluating the mechanical performance of the panels.
The density of wood-based panels can vary depending on raw material properties and production parameters. It has been reported that variations in density and density profiles in commercial particleboard from different manufacturers are related to production conditions (Korai 2024; Korai and Miyatake 2023; Rezanezhad Divkolaei et al. 2025). In this study as well, it is believed that the density differences observed among manufacturers may stem from variations in raw materials and production conditions.
The formaldehyde emission values for commercial E1 and E2 class particleboards are presented in Table 1. Significant differences in formaldehyde emissions were found among manufacturers within both board classes at a 95% confidence level (p < 0.05). According to the results of the independent samples t-test, statistically significant differences were found between the average formaldehyde emission values of E1 and E2 class particleboards (p < 0.05). The average formaldehyde emission values of E1 class particleboards were found to be lower than those of E2 class particleboards. However, the formaldehyde emission values of all commercial particleboards examined fell within the accepted limit values for their respective emission classes (TS EN ISO 12460-5 2016).
It was expected that E1-class particleboards would exhibit lower formaldehyde emission values compared to E2-class boards. Recent studies indicate that the use of low-molecular-weight resins, formaldehyde binders, and alternative adhesive systems reduces formaldehyde emissions in wood-based panels (Kristak et al. 2023; Jiang et al. 2023; Yang et al. 2023a). The fact that all commercial E1 and E2 class particleboards used in the study met the emission class values specified by the standards demonstrates that low-formaldehyde-emitting boards can be produced in commercial manufacturing today. The data distributions for MC, density, and formaldehyde emission values are shown as boxplots in Fig. 6.
Fig. 6. Boxplots showing the physical properties of commercial E1 and E2 particleboards: (a) MC, (b) density, and (c) formaldehyde emission. Boxes represent the interquartile range (Q1 to Q3), the horizontal line indicates the median, whiskers represent the minimum and maximum values excluding outliers, and * indicates a statistically significant difference (p < 0.05)
When the panel’s MC, density, and formaldehyde emission data are evaluated together, it is observed that commercially produced particleboard generally exhibits similar performance, although differences depending on the manufacturer emerge in certain properties. The boxplots presented in Fig. 6 also visually support this variability. The results obtained necessitate evaluating the panels not only in terms of their physical properties but also in terms of their mechanical properties, which provide information about their load-bearing capacity. For this reason, the mechanical properties of commercially available E1 and E2 class particleboards are evaluated in the remainder of this article.
Mechanical Properties
The mean values and descriptive statistics for the MOR, MOE, and IB of commercial E1 and E2 class particleboards are presented in Table 2.
Table 2. MOR, MOE, and IB Values for Commercial E1 and E2 Particleboards (N mm⁻²)
The results of the one-way ANOVA showed that, when classes E1 and E2 were evaluated separately, significant differences in MOR were observed among the manufacturers. In contrast, the independent samples t-test revealed no significant difference between the mean MOR values of the E1 and E2 classes of particleboard (p > 0.05). The highest MOR was determined to be 18.13 N/mm² for manufacturer E2-1, while the lowest value was 12.65 N/mm² for manufacturer E2-2. Considering the minimum MOR requirement of 11.0 N/mm² specified for 18-mm-thick P2 (Board for interior fitments (including furniture) for use in dry conditions) particleboards in the TS EN 312 (2012) standard, regardless of the intended use of the boards, it is observed that all commercial boards examined meet this requirement.
MOR can be influenced by production variables such as panel density, particle geometry, density profile, raw material properties, and pressing conditions (Benthien and Ohlmeyer 2020; Dukarska et al. 2022; Baharuddin et al. 2023; Korai 2024; Taquetti et al. 2023). Scharf et al. (2023) also highlighted the effect of the resin system and production parameters on mechanical performance. In this study, it is considered that the differences in MOR observed among manufacturers may also stem from variations in raw materials and production conditions. The findings reveal that commercial panels meeting the same standard requirements can exhibit different mechanical performance across manufacturers.
It was determined that the values of the MOE varied at a statistically significant level across manufacturers (p < 0.05). Furthermore, the results of the independent samples t-test showed a statistically significant difference between the average MOE values of E1 and E2 class particleboards (p < 0.05). The highest MOE was found in the boards from manufacturer E2-1, while the lowest value was found in the boards from manufacturer E2-2. Considering that, according to the TS EN 312 (2012) standard, the MOE for 18-mm-thick P2-class particleboards must be at least 1800 N/mm², it is evident that all commercial particleboards examined met this requirement.
The MOE can be influenced by various production variables, such as panel density, density profile, particle size, adhesive system, and pressing conditions (Benthien and Ohlmeyer 2020; Baharuddin et al. 2023; Wong et al. 2003; Engehausen et al. 2024). However, it has also been reported that the effect of these variables on the MOE may vary depending on the panel composition and production conditions (Bekhta et al. 2025). The significant difference identified in this study between E1 and E2 class commercial particleboards demonstrates that differences in production and composition among manufacturers can be reflected in mechanical stiffness.
Upon examining the IB values, statistically significant differences were identified among manufacturers. Furthermore, the results of the independent samples t-test indicated a statistically significant difference between the mean IB values of E1 and E2 class commercial particleboard (p < 0.05). The highest IB was 0.76 N/mm² for panels from manufacturer E2-1, while the lowest value was 0.38 N/mm² for panels from manufacturer E1-2. According to the TS EN 312 (2012) standard, the minimum value specified for 18-mm-thick P2-class particleboards is 0.35 N/mm². Considering the IB, it is observed that all commercial particleboards examined meet this minimum value.
IB strength is an important mechanical property that indicates the quality of bonding in the core layer of particleboard and can be influenced by the adhesive system, particle geometry, board density, and production conditions (Benthien and Ohlmeyer 2020; Barbu et al. 2021; Bekhta et al. 2021; Baharuddin et al. 2023). It has also been reported that different adhesive systems, particle size, and raw material properties can cause variations in IB strength (Scharf et al. 2023; Engehausen et al. 2024; Gößwald et al. 2024). The significant differences identified in this study between manufacturers and between E1 and E2 class panels (p<0.05) indicate that variations in commercial production conditions can affect IB performance.
However, the fact that all panels met the minimum value specified in TS EN 312 (2012) reveals that commercial products from different manufacturers can exhibit varying levels of IB performance while still meeting the standard requirements. The distribution of mechanical properties for commercial E1 and E2 class particleboards and the variability among groups are visually presented in Fig. 7 using boxplots.
Fig. 7. Boxplots of the mechanical properties of commercial E1 and E2 particleboards: (a) MOR, (b) MOE, and (c) IB. The boxplots represent the median, interquartile range, and minimum and maximum values. The asterisk (*) indicates a statistically significant difference between E1 and E2 particleboards (p < 0.05).
Fig. 8. Pearson’s correlation heatmap illustrating the relationships among the physical (MC, density, and formaldehyde emission) and mechanical (MOR, MOE, and IB) properties of commercial E1 and E2 particleboards. The lower triangular matrix displays Pearson’s correlation coefficients (r), while the upper triangle is omitted for clarity. Positive correlations are shown in red and negative correlations in blue, with color intensity representing the strength of the relationship. Asterisks (*) indicate statistically significant correlations (p < 0.05).
Changes in the physical and mechanical properties of commercial E1 and E2 grade particleboard, as well as the differences between the groups, are presented visually using boxplots. At the same time, evaluating the relationships among the physical and mechanical properties of the boards is important for understanding their overall performance. For this reason, the linear relationships between physical properties (MC, density, and formaldehyde emission) and mechanical properties (MOR, MOE, and IB) were examined using Pearson’s correlation analysis. The correlation coefficients obtained were visualized as a heat map in Fig. 8 to more clearly illustrate the direction and strength of the relationships.
The Pearson’s correlation analysis shown in Fig. 8 reveals the linear relationships between the physical and mechanical properties of commercial E1 and E2 grade particleboard. According to the analysis results, positive and negative correlations of varying degrees were identified between the physical and mechanical properties. However, only three pairs of variables showed a statistically significant relationship (p < 0.05). A moderate, negative, and statistically significant relationship (r = −0.55) was found between MC and formaldehyde emissions. This indicates that an increase in the equilibrium moisture content of the panels was accompanied by a decrease in the measured formaldehyde emission values. Similarly, Zhang et al. (2022) noted that formaldehyde emissions are significantly influenced by the moisture distribution within the panel, the diffusion mechanism, and environmental conditions. Furthermore, Yang et al. (2023b) emphasized that formaldehyde emissions can vary not only depending on the resin system but also on the panel’s MC and the environment in which it is used. However, Pearson’s correlation analysis reveals a linear relationship between variables. This analysis does not directly indicate a cause-and-effect relationship. Therefore, the combined effect of the resin system, panel structure, production parameters, and environmental conditions must be evaluated when interpreting a negative correlation (Almeida et al. 2025).
A positive and significant correlation (r = 0.61) was found between density and IB. This result indicates that an increase in panel density may positively affect IB by increasing the contact area between wood chips and promoting bond formation among them. Furthermore, recent studies indicate that IB is not solely dependent on average panel density but is also influenced by production parameters such as density profile, chip geometry, surface-to-core ratio, and resin distribution (Korai and Miyatake 2023; Korai 2024). This indicates that the positive correlation identified in the current study is consistent with the mechanical behavior reported in the literature.
Similarly, a significant and positive relationship (r = 0.60) was found between MOR and IB. This finding indicates that stronger internal bonds within the panel positively affect not only internal bond performance but also mechanical behavior under bending loads. Recent literature studies indicate that a reduction in voids within the panel structure and increased homogeneous bonding between chips jointly improve both MOR and IB (Taquetti et al. 2023). Therefore, the MOR-IB correlation identified in the current study supports the decisive role of the panel’s internal structural integrity in its mechanical performance.
However, although positive correlations were observed between density and MOR (r = 0.44) and between density and MOE (r = 0.27), these relationships were not found to be statistically significant (p > 0.05). This result indicates that mechanical performance in commercial particleboard cannot be explained by a single property, such as average density. The literature indicates that MOR and MOE values are significantly influenced not only by panel density but also by particle size and shape, surface and core density distribution, resin system, and production parameters (Camlibel 2023; Almeida et al. 2025). Furthermore, studies on low-formaldehyde-emitting particleboards indicate that changes in production parameters can simultaneously affect both emission behavior and mechanical properties (Ergun et al. 2025). Therefore, the positive but statistically insignificant relationships observed in the current study between density and MOR and MOE can be explained by the multivariate nature of mechanical properties in commercial panels. Overall, Pearson’s correlation analysis revealed that the relationships between density, IB, and MOR are more decisive in terms of panel structural integrity. Conversely, it demonstrated that density alone is not sufficient to explain all mechanical properties. In general, the fact that the differences between E1 and E2 classes do not manifest in all properties indicates that the emission class is not, on its own, a sufficient indicator of panel performance. Therefore, when evaluating the performance of commercial particleboard, it is necessary to consider not only the emission class but also the relationships between manufacturer variations and panel properties.
In future studies, a combined evaluation of the physical, mechanical, and formaldehyde emission properties of commercial particleboard with different thicknesses and usage classes will contribute to a more comprehensive understanding of product performance. Furthermore, the analysis of production parameters, such as panel density profile, particle geometry, and resin content, using multivariate statistical methods will enable a more detailed explanation of the key factors determining panel performance.
CONCLUSIONS
- The physical, mechanical, and formaldehyde emission properties of 18-mm-thick commercial E1 and E2 class particleboards produced by different manufacturers in Turkey were compared. It was determined that all boards examined met the minimum performance criteria specified in the relevant standards.
- No statistically significant difference was found between E1 and E2 class commercial particleboards in terms of moisture content (MC) and modulus of rupture (MOR). However, statistically significant differences were detected between the two emission classes regarding density, formaldehyde emission, modulus of elasticity (MOE), and internal bond (IB) strength. The fact that the differences between E1 and E2 classes do not manifest in all characteristics indicates that the emission class is not, on its own, a sufficient indicator of panel performance.
- As a result of the Pearson’s correlation analysis, a moderate and negative relationship was found between MC and formaldehyde emissions; positive and statistically significant relationships were found between density and IB, as well as between IB and MOR. In contrast, the relationships between density and MOR, and between density and MOE, were not statistically significant.
- The findings reveal that the mechanical performance of commercial particleboard cannot be explained solely by board density, and that IB is an important performance indicator reflecting the board’s structural integrity.
- Boxplots and a Pearson’s correlation heat map visually illustrated the distribution of physical and mechanical properties and the relationships among the variables. These maps and plots complemented the classical statistical analyses and contributed to a more comprehensive interpretation of the results.
- This study presents comparable experimental data on the performance of commercial E1 and E2 grade particleboard produced in Turkey. Significant differences were identified between the E1 and E2 grades in certain physical and mechanical properties. The findings indicate that the performance of commercial particleboard cannot be explained solely by emission class or density.
- In future studies, comparing the physical, mechanical, and emission properties of commercial particleboard panels of various thicknesses and use classes—as well as panels produced using low- or ultra-low-formaldehyde-emitting and formaldehyde-free resin systems—with the current results could contribute to a more comprehensive evaluation of product performance and the feasibility of low-emission alternatives.
- Furthermore, investigating the effects of production variables—such as board density profile, chip geometry, resin content, and resin type—on the technological properties and formaldehyde emissions of the boards using multivariate statistical methods could facilitate a more detailed assessment of the key factors determining performance and of low-emission alternatives.
REFERENCES CITED
Almeida, M. L., Gonçalves, F. D., Martins, J. M., Magalhães, F. D., Ramos, R. M., and Carvalho, L. H. (2025). “Addressing formaldehyde emissions in wood-based panels: Evaluation of production processes, measurement strategies, and novel solutions,” The Journal of Adhesion 101(10), 1252-1274. https://doi.org/10.1080/00218464.2024.2447718
Baharoğlu, M., Nemli, G., Sarı, B., Bardak, S., and Ayrılmış, N. (2012). “The influence of moisture content of raw material on the physical and mechanical properties, surface roughness, wettability, and formaldehyde emission of particleboard composite,” Composites Part B: Engineering 43(5), 2448-2451. https://doi.org/10.1016/j.compositesb.2011.10.020
Baharuddin, M. N. M., Zain, N. M., Harun, W. S. W., Roslin, E. N., Ghazali, F. A., and Som, S. N. M. (2023). “Development and performance of particleboard from various types of organic waste and adhesives: A review,” International Journal of Adhesion and Adhesives 124, article 103378. https://doi.org/10.1016/j.ijadhadh.2023.103378
Barbu, M. C., Montecuccoli, Z., Förg, J., Barbeck, U., Klímek, P., Petutschnigg, A., and Tudor, E. M. (2021). “Potential of brewer’s spent grain as a potential replacement of wood in PMDI, UF or MUF bonded particleboard,” Polymers 13(3), article 319. https://doi.org/10.3390/polym13030319
Bekhta, P., Noshchenko, G., Réh, R., Kristak, L., Sedliačik, J., Antov, P., Mirski, R., and Savov, V. (2021). “Properties of eco-friendly particleboards bonded with lignosulfonate-urea-formaldehyde adhesives and PMDI as a crosslinker,” Materials 14(17), article 4875. https://doi.org/10.3390/ma14174875
Bekhta, P., Ráheľ, J., Pipíška, T., Nociar, M., Leiter, L. M., and Rousek, R. (2025). “Properties of particleboards made from mixture of oversized fibers from MDF waste process and wood particles of Norway spruce (Picea abies),” Wood Material Science & Engineering 20(3), 571-579. https://doir.org/10.1080/17480272.2024.2362753
Benthien, J. T., and Ohlmeyer, M. (2020). “Effects of flat-shaped face layer particles and core layer particles of intentionally greater thickness on the properties of wood-reduced particleboard,” Fibers 8(7), article 46. https://doi.org/10.3390/fib8070046
Calvez, I., Garcia, R., Koubaa, A., Landry, V., and Cloutier, A. (2024). “Recent advances in bio-based adhesives and formaldehyde-free technologies for wood-based panel manufacturing,” Current Forestry Reports 10(5), 386-400. https://doi.org/10.1007/s40725-024-00227-3
Camlibel, O. (2023). “Influence of the multiday and continuous hot press on the physical, mechanical and formaldehyde emission properties of the particleboard,” Maderas. Ciencia y Tecnología 25(7), 1-14. https://doi.org/10.4067/S0718-221X2023000100407
Dukarska, D., Rogoziński, T., Antov, P., Kristak, L., and Kmieciak, J. (2022). “Charac-terisation of wood particles used in the particleboard production as a function of their moisture content,” Materials 15(1), article 48. https://doi.org/10.3390/ma15010048
Engehausen, N., Benthien, J. T., and Lüdtke, J. (2024). “Influence of particle size on the mechanical properties of single-layer particleboards,” Fibers 12(4), article 32. https://doi.org/10.3390/fib12040032
Ergun, M. E., Koyuncu, F., Istek, A., and Özlüsoylu, İ. (2025). “Reducing formaldehyde emissions and enhancing performance of particleboards through the incorporation of activated carbon produced from Scots pine wood residues,” Biofuels, Bioproducts and Biorefining 19(6), 1875-1886. https://doi.org/10.1002/bbb.2788
Food and Agriculture Organization of the United Nations (2025). “FAOSTAT: Forestry production and trade,” FAO, https://www.fao.org/faostat/en/#data/FO, Accessed 22 Dec 2023.
Ghani, A., Ashaari, Z., Lee, S. H., Saifulazry, S., Ahamad, N., A’tiyah, F., and Lee, C. L. (2022). “Amine compounds post-treatment on formaldehyde emission and properties of urea formaldehyde bonded particleboard,” Physical Sciences Reviews 9(1), 63-74. https://doi.org/10.1515/psr-2022-0075
Gößwald, J., Barbu, M. C., Tudor, E. M., and Král, P. (2024). “Leveraging spruce bark particle morphology for enhanced internal bonding in particleboard production,” Polymers 16(21), article 2988. https://doi.org/10.3390/polym16212988
Gumus, N., Doganci, E., and Aytac, A. (2024). “Evaluations of the effects of different flame retardants combinations on particleboards produced using urea–formaldehyde resin,” European Journal of Wood and Wood Products 82(3), 747-759. https://doi.org/10.1007/s00107-024-02054-6
IMARC Group. (2026). “Particle board market size, share, trends and forecast by application, sector, and region, 2026–2034,” IMARC Group, Retrieved from: https://www.imarcgroup.com/particle-board-market, 26 June 2026.
Janiszewska-Latterini, D., and Pizzi, A. (2023). “Application of liquefied wood products for particleboard manufacturing: A meta-analysis review,” Current Forestry Reports 9(4), 291-300. https://doi.org/10.1007/s40725-023-00192-3
Jiang, S., Duan, Z., Liu, S., Du, G., Wang, S., Zhou, X., Yang, Z., and Li, T. (2023). “Long-chain polyamine-glyoxal wood adhesive: Formaldehyde-free, green synthesis, and ultra-performances,” ACS Sustainable Chemistry & Engineering 11(35), 13209-13221. https://doi.org/10.1021/acssuschemeng.3c04378
Korai, H. (2024). “Analysis of the density profile and bending properties of commercial particleboard,” Journal of the Indian Academy of Wood Science 21(2), 255-264. https://doi.org/10.1007/s13196-024-00344-3
Korai, H., and Miyatake, A. (2023). “Effect of outer core-layer density on bending properties of commercial particleboard,” Wood Material Science & Engineering 18(3), 943-951. https://doi.org/10.1080/17480272.2022.2091950
Kord, B., Movahedi, F., Adlnasab, L., and Ayrilmis, N. (2022). “Effect of novel scavengers based on phenolic compounds on formaldehyde emission and physical-mechanical properties of particleboard,” Wood Material Science and Engineering 17(6), 954-964. https://doi.org/10.1080/17480272.2021.1978542
Kristak, L., Antov, P., Bekhta, P., Lubis, M. A. R., Iswanto, A. H., Reh, R., Sedliacik, J., Savov, V., Taghiyari, H. R., Papadopoulos, A. N., Pizzi, A., and Hejna, A. (2023). “Recent progress in ultra-low formaldehyde emitting adhesive systems and formaldehyde scavengers in wood-based panels: A review,” Wood Material Science & Engineering 18(2), 763-782. https://doi.org/10.1080/17480272.2022.2056080
Ma, Y., Kou, Z., Hu, Y., Zhou, J., Bei, Y., Hu, L., Huang, Q., Jia, P., and Zhou, Y. (2023). “Research advances in bio-based adhesives,” International Journal of Adhesion and Adhesives 126, article 103444. https://doi.org/10.1016/j.ijadhadh.2023.103444
Mirindi, D. (2024). “A review of particleboard development and performance using non-toxic and biodegradable adhesives,” International Journal of Engineering Trends and Technology 72(5), 252-260. https://doi.org/10.14445/22315381/IJETT-V72I5P126
Papadopoulou, E., and Chrissafis, K. (2017). “Particleboards from agricultural lignocellulosics and biodegradable polymers prepared with raw materials from natural resources,” in: Natural Fiber-reinforced Biodegradable and Bioresorbable Polymer Composites, A. K.-T. Lau and A. P.-Y. Hung (eds.), Woodhead Publishing, Sawston, UK, pp. 19–30. https://doi.org/10.1016/B978-0-08-100656-6.00002-9
Rezanezhad Divkolaei, M., Shalbafan, A., and Thoemen, H. (2025). “Influence of panel density on the characteristics of novel multifunctional particleboard,” Wood Material Science and Engineering 20(1), 205-216. https://doi.org/10.1080/17480272.2024.2338202
Ryu, D. Y., Shimohara, T., Nakabayashi, K., Miyawaki, J., Park, J. I., and Yoon, S. H. (2019). “Urea/nitric acid co-impregnated pitch-based activated carbon fiber for the effective removal of formaldehyde,” Journal of Industrial and Engineering Chemistry 80, 98-105. https://doi.org/10.1016/j.jiec.2019.07.036
Scharf, A., Popescu, C. M., Dernegård, H., Oja, J., Ormondroyd, G., Medved, S., Sandberg, D., and Jones, D. (2023). “Particleboards bonded by an imidazole-based adhesive system,” Materials 16(22), article 7201. https://doi.org/10.3390/ma16227201
Taquetti, V. B., Silva, V. V., Chaves, I. L. S., Oliveira, R. G. E., Maffioletti, F. D., Ferreira, G., Mendonça, J. P. C., Silva, E. S. G., and Gonçalves, F. G. (2023). “Performance of eucalypt particleboard with the addition of farm waste,” Heliyon 9(12), article e22760. https://doi.org/10.1016/j.heliyon.2023.e22760
Thybring, E. E., and Fredriksson, M. (2023). “Wood and moisture,” in: Springer Handbook of Wood Science and Technology, P. Niemz, A. Teischinger, and D. Sandberg (eds.), Springer, Cham, Switzerland, pp. 355-397. https://doi.org/10.1007/978-3-030-81315-4_7
TS 642 ISO 554 (1997). “Standard atmospheres for conditioning and/or testing; Specifications,” Turkish Standards Institution, Ankara, Turkey.
TS EN 310 (1999). “Wood-based panels – Determination of modulus of elasticity in bending and of bending strength,” Turkish Standards Institution, Ankara, Turkey.
TS EN 312 (2012). “Particleboards – Specification,” Turkish Standards Institution, Ankara, Turkey.
TS EN 319 (1999). “Particleboards and fibreboards – Determination of tensile strength perpendicular to the plane of the board,” Turkish Standards Institution, Ankara, Turkey.
TS EN 322 (1999). “Wood-based panels – Determination of moisture content,” Turkish Standards Institution, Ankara, Turkey.
TS EN 323 (1999). “Wood-based panels – Determination of density,” Turkish Standards Institution, Ankara, Turkey.
TS EN ISO 12460-5 (2016). “Wood-based panels – Determination of formaldehyde release-Part 5: Extraction method (called the perforator method),” Turkish Standards Institution, Ankara, Turkey.
Wong, E. D., Yang, P., Zhang, M., Wang, Q., Nakao, T., Li, K. F., and Kawai, S. (2003). “Analysis of the effects of density profile on the bending properties of particleboard using finite element method (FEM),” European Journal of Wood and Wood Products 61(1), 66-72. https://doi.org/10.1007/s00107-002-0350-9
Yang, G., Gong, Z., Luo, X., Chen, L., and Shuai, L. (2023a). “Bonding wood with uncondensed lignins as adhesives,” Nature 621, 511-515. https://doi.org/10.1038/s41586-023-06507-5
Yang, Y., Zhang, Z., Zhang, L., Song, F., Ren, Y., Zhang, X., Zhang, J., Liew, R. K., Foong, S. Y.,Chong, W. W. F., Lam, S. S., Verma, M., Ng, H. S., Sonne, C., and Ge, S. (2023b). “Recent advances in the control of volatile organic compounds emissions from indoor wood-based panels: A comprehensive review,” Science of The Total Environment 884, article 163741. https://doi.org/10.1016/j.scitotenv.2023.163741
Younesi-Kordkheili, H. (2024). “Reduction of formaldehyde emission from urea-formaldehyde resin by maleated nanolignin,” International Journal of Adhesion and Adhesives 132, article 103677. https://doi.org/10.1016/j.ijadhadh.2024.103677
Zhang, Y., Xu, N., Bai, Y., Liu, J., Guo, Z., and Niu, Y. (2022). “Comparison of multidimensional mass transfer models of formaldehyde emissions originating from different surfaces of wood-based panels,” Science of the Total Environment 848, article 157367. https://doi.org/10.1016/j.scitotenv.2022.157367
Article submitted: July 30, 2026; Peer review completed: August 29, 2026; Revised version received: September 1, 2026; Accepted: October 7, 2026; Published: October 28, 2026.