Abstract
Thermally modified Scots pine (Pinus sylvestris var. mongolica Litv.) was used as the substrate, while Scots pine and birch (Pinus sylvestris var. mongolica Litv.) were used as dowel materials. Infrared thermography, SEM, GC-MS, and FTIR were employed to investigate the relationships among process parameters, interfacial temperature, and welding performance in rotary friction welding of wood. The interfacial temperature exhibited a three-stage evolution pattern of rapid heating, stabilisation, and cooling-solidification. Rotational speed, feed rate, and dowel-to-hole diameter ratio regulated the interfacial temperature by affecting frictional heat generation efficiency and interaction duration, with each parameter exhibiting an optimal range. An appropriate temperature range (360 to 380 °C) promoted hemicellulose degradation, lignin softening, and flow, and the formation of a dense welded zone after cooling. Birch dowels generated higher interfacial temperatures and bonding strength than Scots pine dowels. The findings indicate that rotary friction welding of wood is a temperature-dominated thermo-mechanical-chemical coupled process, and that optimising process parameters to precisely control interfacial temperature is essential for achieving high-performance adhesive-free joints.
Download PDF
Full Article
Evolution of Interfacial Temperature in Rotary Friction Welding of Wood and Its Influence on the Bonding Mechanism
Jian Zhang,a Yuelong Li,a Hui Jiang,b,* Hai Zhu,a Yao Deng,a Yanfeng Li,c and YuJia Liu c
Thermally modified Scots pine (Pinus sylvestris var. mongolica Litv.) was used as the substrate, while Scots pine and birch (Pinus sylvestris var. mongolica Litv.) were used as dowel materials. Infrared thermography, SEM, GC-MS, and FTIR were employed to investigate the relationships among process parameters, interfacial temperature, and welding performance in rotary friction welding of wood. The interfacial temperature exhibited a three-stage evolution pattern of rapid heating, stabilisation, and cooling-solidification. Rotational speed, feed rate, and dowel-to-hole diameter ratio regulated the interfacial temperature by affecting frictional heat generation efficiency and interaction duration, with each parameter exhibiting an optimal range. An appropriate temperature range (360 to 380 °C) promoted hemicellulose degradation, lignin softening, and flow, and the formation of a dense welded zone after cooling. Birch dowels generated higher interfacial temperatures and bonding strength than Scots pine dowels. The findings indicate that rotary friction welding of wood is a temperature-dominated thermo-mechanical-chemical coupled process, and that optimising process parameters to precisely control interfacial temperature is essential for achieving high-performance adhesive-free joints.
DOI: 10.15376/biores.21.4.11648-11675
Keywords: Rotary friction welding; Wood welding; Interfacial temperature; Process parameters;
Welding mechanism; Heat-treated wood
Contact information: a: College of Mechanical and Electrical Engineering, Northeast Forestry University, No. 26 Hexing Road, Xiangfang District, Harbin, Heilongjiang, China.; b: School of Foreign Languages, Northeast Forestry University, No. 26 Hexing Road, Xiangfang District, Harbin, Heilongjiang, China; c: Qiqihar Heping Heavy Industry Co., Ltd., *Corresponding author: [email protected]
INTRODUCTION
As a natural, green, and low-carbon biomass material, wood is characterised by its environmental friendliness, renewability, and biodegradability. Under the “dual-carbon” strategy, wood is regarded as a natural “carbon-negative” material and is considered one of the most promising alternatives to high-carbon materials such as plastics and steel (Yun 2022). During wood welding, variations in interfacial temperature influence the physicochemical reactions occurring in the process, thereby affecting the final welding performance. A thorough understanding of wood chemistry is essential for elucidating the thermochemical reactions involved in welding, as these reactions govern the bonding mechanisms and ultimately determine the strength of the weld line (Belleville et al. 2019).
The bonding mechanisms of wood welding have been extensively investigated (Pintiaux et al. 2015; Zhang et al. 2015; Hubbe et al. 2018), and are mainly associated with the following aspects: (1) degradation of hygroscopic hemicellulose leading to the formation of soluble sugars, which may further react to become less hygroscopic and form highly branched polysaccharides; (2) generation of free sugars through hemicellulose degradation, which may undergo polymerisation during hot pressing to form adhesive-like substances; (3) thermal softening of the cell-wall matrix, predominantly within lignin, which allows reorganisation into a new matrix with reduced residual stress after pressing; and (4) cross-linking reactions occurring between lignin and carbohydrate polymers and/or among carbohydrate polymers.
Interfacial temperature evolution during wood welding plays a critical role in governing these physicochemical transformations and consequently has a significant influence on the final bonding quality. Xiao et al. (2018) employed fibre-optic sensors to measure the temperature variation in Pinus sylvestris var. mongolica. Their results indicated that the internal temperature evolution during microwave treatment generally followed two distinct patterns. In the first pattern, the temperature development could be divided into three stages: heating, isothermal stabilisation, and rapid temperature rise. In the second pattern, two stages were observed: heating and isothermal stabilisation. With increasing microwave power, both the maximum temperature (MT) and the temperature rise rate (RTI) increased. Yang et al. (2022) conducted welding studies using temperature monitoring combined with infrared spectroscopy. The temperature measurements showed that the peak temperature of the bamboo-tenon welding layer reached 337 °C, whereas that of the wood-tenon welding layer was 292 °C. Compared with the wood-tenon welding layer, the bamboo-tenon layer exhibited a faster heating rate, a higher temperature peak, and a longer duration of high-temperature retention.
A deeper understanding of the fundamental mechanisms underlying wood welding requires systematic investigation of the compositional transformations occurring during the process, in which temperature plays a decisive role in altering the content and structure of wood constituents. Scott et al. (2005) employed Fourier transform infrared spectroscopy (FTIR) and reported that an increase in the peak intensity at 1335 cm⁻¹ could be used to identify the cleavage mechanism of ether linkages. Gedara et al. (2021) investigated the thermal degradation mechanism of β-ether bonds using phenethyl phenyl ether as a lignin model compound, demonstrating that a key step in lignin pyrolysis is the homolytic cleavage of α- and β-alkyl aryl ether bonds. Li et al. (2007) conducted steam treatment of lignin isolated from poplar and analysed the resulting structural changes using nuclear magnetic resonance (NMR) and size-exclusion chromatography, thereby revealing both depolymerisation and condensation reactions of lignin. Zor et al. (2020) examined the water resistance of thermally modified wood species, including mulberry, ash, tulipwood and ayous, and found that the degree of thermal modification and the intrinsic properties of the wood significantly influenced the water absorption behaviour of the welded seam. Amirou et al. (2020) further reported that thermal modification improves dimensional stability by reducing hygroscopicity and water uptake; however, it may also lead to reduced bondability in certain applications.
Thermal modification can influence subsequent welding performance, but its effects depend on the wood species, treatment conditions, and welding parameters. Zhang et al. (2025) investigated rotary friction welding of heat-treated Scots pine and reported improved joint performance under selected conditions compared with untreated material. In contrast, Župčić et al. (2023) reported reduced pull-out forces for dowels welded into thermally modified substrates. These findings show that the influence of thermal modification on weldability is condition-dependent and cannot be inferred solely from improvements in dimensional stability.
Previous investigations of rotary dowel welding have examined the relationships among processing parameters, temperature development, and joint performance. Belleville et al. (2013) investigated interface temperatures and withdrawal strength for sugar maple and yellow birch. Župčić et al. (2021) examined welding temperatures and pull-out performance, while Zhang et al. (2025) investigated temperature distributions in relation to welding depth, time, and dowel pretreatment. Together with the studies on thermally modified wood discussed above, these investigations provide a basis for examining how material selection and processing conditions affect thermal histories and joint formation.
The present study examined the temperature evolution during rotary friction welding of Scots pine and birch dowels into thermally modified Scots pine substrates. Infrared thermography was combined with scanning electron microscopy (SEM), gas chromatography-mass spectrometry (GC–MS), and Fourier transform infrared (FTIR) spectrometry to investigate the associations among welding parameters, measured thermal histories, interfacial morphology, and chemical changes in the sampled welded material. Particular attention is given to differences between the two dowel materials under the investigated conditions.
Quantitative understanding of interfacial temperature evolution and its relationship with bonding performance during rotary friction welding of wood has remained limited, particularly for thermally modified Scots pine. Previous studies have mainly focused on welding parameters and mechanical performance, while the coupling between interfacial temperature, material transformation, and joint formation has received less attention. Therefore, this study investigated the interfacial temperature evolution of thermally modified Scots pine during rotary friction welding and examines its relationship with welding parameters, joint strength, and interfacial microstructural changes. The specific objectives were to clarify the temperature evolution during welding, determine the influence of key welding parameters on joint performance, and elucidate how thermally induced material changes contribute to interfacial bonding.
EXPERIMENTAL
Materials
Thermally modified Scots pine ([pine scientific name]) was used as the substrate, with dimensions of 100 mm × 50 mm × 20 mm (length × width × thickness). Through-holes with a diameter of 8 mm were pre-drilled in the specimens. Scots pine of the same species and birch ([birch scientific name]) were selected as dowel materials. The dowels were smooth cylindrical rods with their longitudinal axes parallel to the grain, diameters of 10, 11, 12, and 13 mm, and a length of 100 mm.
To ensure welding stability, the welding ends of all dowels were machined with a 45° chamfer, with a chamfer length of 8 mm. Prior to welding, the moisture contents of both the dowels and the base material were adjusted to 7 to 10%. Supplementary moisture-content measurements were performed on unwelded material retained from the same batches as the experimental substrates and dowels. Ten independent specimens were examined for each of the three material groups: thermally modified Scots pine, Scots pine dowel material, and birch dowel material. Measurements were conducted at 20 ± 2 °C using a J-2000 pin-type resistance moisture meter (Delmhorst Instrument Co., USA). Three readings were taken at separate locations on each specimen, and their mean was used as the specimen-level meter reading. The electrode configuration, species setting, and temperature setting were recorded. The meter readings were compared with oven-dry moisture contents determined from the same specimens. This comparison was particularly important for the thermally modified material, for which the applicability of an untreated-wood calibration could not be assumed.
Significant differences exist between the two dowel materials in terms of density, mechanical properties, and thermophysical parameters. The relevant properties are presented in Table 1. These differences provide a basis for subsequent analysis of the interfacial temperature response and welding mechanism under different dowel materials. The detailed geometry of the welded specimens and the through-hole configuration is illustrated in Fig. 1.
Fig. 1. Schematic illustration of the welded specimen and its through-hole configuration
Table 1. Specific Parameters of Each Material
Thermal Modification and Conditioning of the Substrate
Thermal modification refers to the process in which wood is heated within a temperature range of 150 to 260 °C in media such as steam, air (oxygen-deficient conditions), nitrogen, or vegetable oil, producing so-called “thermally modified wood”. The procedure is generally divided into three stages. The first stage is drying: the fuel in the combustion chamber of the thermal modification equipment is ignited, and the temperature is slowly increased over 4 to 6 h to heat the dried wood to 103 °C, ensuring an oven-dry condition. The second stage is the heating and treatment stage: airflow is adjusted and steam is injected to raise the wood temperature to the target treatment level within 3 to 4 h, followed by an isothermal holding period. During this stage, the gas composition of the mixed flue gas-including oxygen, CO₂, CO, and steam-must be regulated, while the relative humidity of the treatment environment is controlled. Under a constant treatment temperature, heating is maintained for a further 3 to 4 h. The third stage is cooling: the biomass fuel is extinguished and the wood is allowed to cool naturally under sealed conditions until the temperature decreases below 100 °C. Subsequently, steam is introduced for moisture conditioning to adjust the moisture content to 4 to 6%. Finally, the wood is discharged from the chamber at approximately 40 °C, completing the entire treatment process.
Experimental Design
Owing to the significant differences in density, cellular structure, and thermophysical properties between the two dowel materials, their optimal welding parameters were not identical. In this study, the previously determined optimal welding parameters for each dowel material were adopted as the baseline conditions. For birch dowels, the optimal parameters were a hole-to-dowel diameter ratio of 12/8, a rotational speed of 2500 r/min, and a feed speed of 25 mm/s. For Scots pine dowels, the corresponding optimal parameters were a hole-to-dowel diameter ratio of 12/8, a rotational speed of 3000 r/min, and a feed speed of 25 mm/s. Based on these baseline conditions, the effects of the hole-to-dowel diameter ratio, rotational speed, and feed speed on the interfacial temperature evolution during rotary friction welding were systematically investigated using the single-factor method, while the remaining parameters were kept constant. All experiments were conducted under identical substrate conditions, and each parameter combination was repeated three times to minimize experimental uncertainty.
Fig. 2. Specimen configuration for infrared temperature monitoring: (a) photograph of the specimen with a stepped lateral observation opening; (b) schematic showing the infrared viewing direction and the exposed welding region accessible through the opening
A stepped lateral observation hole was machined into the substrate to provide optical access to the welding region (Fig. 2). The outer and inner sections had diameters of 14 and 6 mm, respectively. The outer section extended 15 mm from the lateral surface, and the inner section extended a further 8 mm towards the welding hole. The centre of the observation opening was located 10 mm below the dowel-entry surface. This configuration exposed part of the welding region for infrared observation while altering the local boundary conditions.
Temperature was monitored using a FOTRIC 616C-L30 infrared thermal imaging camera (Fig. 3). The measurement range was set to −20 to 550 °C, the camera-to-specimen distance was 300 mm, and the ambient temperature was approximately 25 °C. A constant emissivity setting of 0.95 was used as a provisional assumption, rather than a specimen-specific calibrated value. Radiometric images were recorded at 30 frames/s. The region of interest encompassed the visible welding region within the inner opening, excluding the surrounding hole walls and background. Temperature histories were constructed from the maximum apparent temperature within this region in each frame. Recording covered welding and subsequent cooling. Uncertainty associated with the assumed emissivity and the observation opening was acknowledged when interpreting the temperatures.
Fig. 3. FOTRIC 616C-L30 infrared thermal imaging camera
Experimental Apparatus for Rotary Friction Welding of Wood
The welding experimental platform is shown in Fig. 4. Prior to welding, the base material was firmly clamped to the platform using a bench vice. Through-holes were pre-drilled on the specimen surface, and the wood chips inside the holes were carefully removed using a brush to ensure welding quality.
Fig. 4. Rotary friction welding apparatus for wood
During welding, the dowel was secured using a dedicated fixture to guarantee stable operation throughout the process. The required welding parameters were set and adjusted via the control interface. When the spindle drove the dowel to rotate at high speed and fed it into the base material at a specified rate, intense frictional heat was generated instantaneously at the interface. This elevated temperature induced the melting and flow of wood components such as lignin and hemicellulose. As the temperature subsequently decreased, a welded zone was formed, thereby achieving the bonding effect. Detailed data on the welding strength have been presented in the authors’ previous research article (Zhang et al. 2025).
Mechanical Testing Equipment
The mechanical performance of the specimens was evaluated in accordance with GB/T 14018 (2009), with the pull-out resistance of rotary friction welded wood dowel joints being determined. A WDW100 universal testing machine was employed for the tests.
During tensile loading, the specimens were mounted using a specially designed fixture. The upper clamping length was approximately 40 mm, while the lower base material was positioned in close contact with the fixture surface (Fig. 5a). The loading rate was set to 5 mm/min until the dowel was completely pulled out. The pull-out testing fixture is shown in Fig. 5b.
GB/T 14018(2009) was adopted as a reference for the tensile testing procedure and loading configuration, with appropriate modifications to accommodate the geometry of the rotary-friction-welded dowel joint. The effective welded length was 50 mm, while the remaining exposed dowel length was used for gripping and loading. Three specimens were tested for each experimental condition, and all specimens were conditioned to a moisture content of approximately 7 to 10% before testing. Tensile loading was applied using a WDW100 universal testing machine at a displacement rate of 5 mm/min. The displacement was defined as the crosshead displacement during tensile loading, and the maximum load before failure was taken as the joint strength.
Fig. 5. Tensile testing equipment and scanning electron microscopy system
Scanning Electron Microscopy (SEM) Analysis
To more clearly observe the microstructural features of the welded joints and interfaces before and after welding, specimens were sectioned from the welded components. The sampling dimensions were 15 mm × 15 mm × 5 mm (length × width × thickness), as shown in Fig. 6(a). After removing surface dust, the samples were placed in a gold sputtering chamber for metallic coating (Fig. 6(b)) to enhance electrical conductivity and improve imaging quality. A scanning electron microscope was then used to examine the fine microstructural characteristics of the welded joints and interfacial regions, and to analyze the structural changes induced by welding. The observations were conducted using a COXEM EM-30N scanning electron microscope, as shown in Fig. 6(c).
Fig. 6. (a) Welded joint and sampling results, (b) gold sputtering device (ETD-200 ion sputter coater), and (c) COXEM EM-30N scanning electron microscope
Gas Chromatography–Mass Spectrometry (GC–MS) Analysis
Samples were collected from the welded wood specimens after welding. The blackened material on the surface of the welded zone was carefully scraped off using a knife and ground into fine powder with a mortar. The resulting powder was dissolved in chromatographic-grade methanol and subsequently subjected to GC–MS analysis. The GCMS-240 gas chromatography–mass spectrometry system is shown in Fig. 7.
GC-MS analysis was performed to characterize the methanol-extractable components of the wood before and after rotary friction welding. The samples were extracted under identical conditions using the same sample mass, extraction solvent volume, extraction time, and analytical procedure. The GC-MS analysis was conducted using a capillary column with helium as the carrier gas and electron ionization (EI) mode. The detected compounds were identified by comparison with the NIST spectral library, and only compounds with acceptable spectral matching quality and consistent retention behavior were considered for assignment. Blank and replicate analyses were used to assess background interference and analytical repeatability. The relative peak areas were normalized to the total detected peak area and were therefore interpreted as relative compositional changes rather than absolute concentration changes.
To minimize sampling bias, the before- and after-welding samples were collected from comparable wood regions and processed using the same extraction procedure. The GC-MS results showed changes in the relative abundance of several extractable compounds after welding, including the formation or enhancement of some thermally derived products such as furfural.
Fig. 7. GCMS-240 gas chromatography-mass spectrometry (GC-MS) system
Fourier Transform Infrared Spectroscopy (FTIR) Analysis
Fourier transform infrared spectroscopy (FTIR) is a non-destructive analytical technique based on molecular vibrational spectroscopy. Its principle lies in the generation of an interferogram by an interferometer, which is subsequently converted into an infrared absorption spectrum through Fourier transformation. FTIR enables rapid qualitative and quantitative analysis of samples in various forms, providing extensive information on molecular structure and chemical composition.
The FTIR measurements were performed using a Thermo Scientific Nicolet iS50 Fourier transform infrared spectrometer equipped with a diamond ATR accessory. The spectra were collected over the range of 4000 to 400 cm⁻¹ with a spectral resolution of 4 cm⁻¹, and 32 scans were accumulated for each measurement. Before each measurement, a background spectrum was collected under the same instrumental conditions. The samples were collected from the surface layer of the welded region and directly analyzed using the ATR accessory. Three independent specimens were analyzed for each condition. The obtained spectra were subjected to baseline correction and normalization before further comparison.
Prior to testing, samples were collected from the welded zone. The material was ground into powder using a mortar and pestle, and then it was sieved to obtain fine particles to improve measurement accuracy. The prepared powder was placed into the measurement area of the FTIR instrument. The rotating pressing device was operated to compress the sample into a flat pellet, after which spectral acquisition was performed. Infrared spectra with characteristic absorption peaks were obtained, allowing analysis of the compositional changes of wood constituents during the welding process, as shown in Fig. 8.
Fig. 8. FTIR infrared spectroscopy measurement equipment
RESULTS AND DISCUSSION
Interfacial Temperature Monitoring during the Welding Process
Rotary friction welding of wood is characterised by a short processing time and a rapid heating rate. Infrared thermography results indicate that the interfacial temperature exhibited a typical three-stage evolution pattern throughout the welding process, namely “rapid heating – high-temperature stabilisation – cooling and solidification”. The overall welding process is illustrated in Figs. 9 and 10.
Before contact, the displayed apparent temperatures ranged from approximately 17.2 to 25.9 °C (Figs. 9a and 9c), with local spatial variations. The region corresponding to the subsequent welding observation area is marked in Fig. 9. After contact, a pronounced localized hot spot developed in this region (Figs. 9b and 9d). These observations illustrate the onset of localized frictional heating, rather than a uniformly distributed temperature field.
When the welding tool first contacted the wood specimen and friction was generated (Fig. 9(b) and Fig. 9(d)), the interfacial temperature rose rapidly to approximately 75 °C. At this stage, frictional heat began to accumulate locally, resulting in a pronounced single-peak structure in the temperature field, although the heat-affected zone remained limited. The three-dimensional profile shows a steep and narrow temperature peak, suggesting that the generated heat had not yet diffused extensively into the wood.
Fig. 9. Infrared thermography images showing temperature variations at the initial stage of welding and at the moment of contact: (a) temperature distribution before the dowel contacts the base material; (b) temperature distribution when the dowel tip first contacts the base material; (c) three-dimensional temperature data before contact; and (d) three-dimensional temperature data at initial contact. The marked regions identify corresponding observation locations before and after contact.
As friction continued to intensify and the process entered the stable welding stage (Fig. 10(a) and Fig. 10(c)), the interfacial temperature increased sharply. In the present study, the maximum temperature reached approximately 376 °C. At this stage, the combined effects of high-speed rotation and continuous axial compression promoted the softening and partial thermal decomposition of lignin and hemicellulose, thereby contributing to the formation of a dense welded zone. The three-dimensional temperature field exhibited a high and sharply defined peak, indicating that heat was highly concentrated in the vicinity of the welding interface, which is a typical characteristic of rotary friction welding of wood. The measured peak temperature of approximately 376 °C can be compared with published results for rotary dowel welding, provided that differences in measurement methods and processing conditions are considered. At 2500 r/min, Belleville et al. (2013) reported mean peak temperatures of 328.6 °C for sugar maple and 327.3 °C for yellow birch, with maximum recorded values of 380 and 371 °C, respectively. The present value is comparable to the upper recorded temperatures in that study. However, differences in wood species, insertion conditions, joint geometry, and sensor location prevent direct equivalence between the measurements. In particular, the present infrared measurements were obtained through an observation opening and should not be interpreted as the maximum temperature throughout an intact, enclosed interface.
Fig. 10. Infrared thermography images showing temperature evolution during the stable welding stage and the post-welding cooling process: (a) Interfacial temperature reaching the peak value during welding; (b) Temperature reduction process after welding; (c) Three-dimensional temperature data at the peak interfacial temperature; and (d) Three-dimensional temperature data during the cooling stage
After spindle rotation stopped, the interface entered the cooling stage (Fig. 10(b) and Fig. 10(d)), and the measured peak temperature decreased to approximately 257 °C. Although wood has low thermal conductivity, the steep temperature gradient between the narrow heated region and the adjacent cooler material allows heat transfer over short distances. The cessation of frictional heat generation, together with continued conduction and heat loss from exposed surfaces, can therefore explain the decline in local temperature. The remaining hot region indicates residual heat near the interface rather than a separate annealing treatment. The observed cooling does not imply rapid temperature equilibration throughout the specimen.
Following the cessation of rotation, the dowel remained embedded in the substrate while the welded region cooled. Cooling of the thermally mobilized material can contribute to the development of a stable interfacial structure. The recorded temperature history characterizes cooling at the observation region; it does not establish the time required for the entire joint to return to ambient temperature.
The thermograms and corresponding surface temperature profiles describe the thermal evolution of the exposed observation region. The opening may increase convective and radiative heat loss and may also change local contact pressure, material expulsion, and oxygen access. These effects can influence both the actual local temperature and the temperature recorded by the camera. Because the opening-induced disturbance was not independently quantified, the results are interpreted as apparent temperatures of the exposed region rather than measurements of the maximum temperature throughout an intact interface. A common opening geometry improves procedural consistency but does not demonstrate that the measurement bias is identical under all welding conditions.
Influence of Process Parameters on Interfacial Temperature
The interfacial temperature during welding governs the thermal response behavior of lignin, hemicellulose, and cellulose. It serves as a critical intermediate variable linking process parameters to welding quality. Different process parameters affect the welding temperature and its stability by regulating the intensity of frictional heat generation and the duration of high-temperature exposure.
To further clarify the mechanisms responsible for variations in welding strength under different process conditions, it is necessary to monitor the time-dependent evolution of interfacial temperature and to analyze the influence of process parameters on temperature development. In this study, temperature analysis software was used to process and organize the temperature–time data obtained from each experimental group. Meanwhile, the temperature history during welding directly determines the degradation and repolymerization behaviors of lignin, cellulose, and hemicellulose, and the melting and re-solidification of these components ultimately affect the quality of the welded layer. These constituents exhibit different thermal degradation temperature ranges under high-temperature conditions: hemicellulose degrades within 225 to 350 °C, cellulose within 325 to 375 °C, and lignin within 250 to 500 °C. Therefore, the high-temperature environment generated during welding can induce distinct thermal responses in each component.
Due to its highly branched structure, hemicellulose is more susceptible to thermal degradation during welding, producing volatile compounds. In contrast, cellulose exhibits relatively high thermal stability; when the welding temperature does not reach its degradation threshold or the exposure time is insufficient, cellulose undergoes little degradation. However, within the range of 220 to 240 °C, disruption of its crystalline structure may occur, leading to a reduction in the degree of polymerization. As for lignin, as a thermoplastic polymer, it does not possess a distinct melting point but exhibits a glass transition temperature. Under heating during welding, lignin softens and flows.
The welding process is characterized by the softening and viscous flow of molten lignin, the thermal degradation of hemicellulose, and the bending and entanglement of cellulose fibers. Upon completion of welding and subsequent cooling, the mobilized hemicellulose- and lignin-derived substances interpenetrate and become intertwined within the cellulose framework, ultimately forming the welded zone.
Under the optimal welding conditions for the two dowel materials, single-factor experiments were conducted by varying one parameter at a time to investigate the effects of process parameters on welding temperature. The peak interfacial temperatures under the optimal conditions were 367.4 °C for birch dowels and 365.3 °C for Scots pine dowels.
Effect of Dowel-to-Hole Diameter Ratio on Interfacial Temperature
Under constant rotational speed and feed rate, the dowel-to-hole diameter ratio exerts a significant influence on the welding temperature. With an increase in the diameter ratio, the interfacial temperature initially rises and reaches a maximum at a moderate ratio, after which it tends to stabilize or slightly decrease. This indicates that a larger diameter ratio does not necessarily lead to a higher welding temperature; instead, an optimal range exists in which frictional heat generation and interfacial material softening act synergistically. The corresponding experimental scheme is presented in Table 2.
Table 2. Experimental Design under Different Dowel-to-Hole Diameter Ratios
As shown in Fig. 11, the overall temperature-time evolution trends of the two dowel materials under different diameter ratios are generally consistent, both exhibiting three typical stages: rapid heating, a high-temperature plateau, and cooling.
Fig. 11. Effects of different dowel-to-hole diameter ratios on welding temperature for (a) Scots pine and (b) birch dowels
During the initial welding period (0 to 2 s), intense friction between the high-speed rotating dowel and the hole wall rapidly converts frictional work into thermal energy, resulting in a sharp increase in interfacial temperature. Subsequently, a high-temperature stabilization stage occurs at approximately 4 to 7 s, during which frictional heat generation and heat transfer/dissipation reach a relative equilibrium. After welding is completed, the interfacial temperature decreases rapidly as rotation stops.
Under identical conditions in which the base material was heat-treated Scots pine, variations in the dowel-to-hole diameter ratio exerted a pronounced influence on the interfacial temperature evolution during rotary friction welding for both Scots pine and birch dowels. The temperature evolution patterns of the two dowel materials were generally consistent across different diameter ratios, with the welding process exhibiting three typical stages: rapid heating, high-temperature stabilization, and subsequent cooling.
For the Scots pine dowel (Fig. 11a), as the diameter ratio increased from 10/8 to 12/8, the maximum interfacial temperature gradually increased. This indicates that an appropriate increase in the diameter ratio improves the frictional contact condition between the dowel and the hole wall, enhances frictional heat generation efficiency per unit time, and thereby promotes a higher interfacial temperature. When the dowel-to-hole diameter ratio was further increased to 13/8, the peak temperature showed a slight decrease. One possible explanation is that excessive dowel diameter relative to the fixed hole diameter increases the interference and may promote excessive material extrusion, local deformation, and unstable frictional contact. Heating a greater amount of material would distribute the generated heat over a larger mass, potentially limiting the temperature rise. However, this explanation remains tentative because the amount of softened material was not quantified. The lower peak temperature alone does not establish whether joint strength increased or decreased. Further investigation combining temperature measurements with mechanical testing is planned to clarify this relationship.
In contrast, the birch dowel (Fig. 11b) exhibited a noticeably higher overall welding temperature than the Scots pine dowel under the same diameter ratios. Birch dowel demonstrated a more pronounced response to changes in the diameter ratio. When the diameter ratio increased from 10/8 to 12/8, the peak interfacial temperature increased significantly, reaching its maximum value at 12/8. With a further increase to 13/8, the welding temperature remained at a relatively high level; however, the increasing trend became less evident and tended to level off.
Effect of Rotational Speed on Interfacial Temperature
Under constant dowel-to-hole diameter ratio and feed rate, rotational speed was found to exert a more pronounced influence on the temperature evolution rate and the stability of the peak temperature during the welding process. With increasing rotational speed, the heating rate during the initial stage of welding increased significantly. However, when the rotational speed became excessively high, the peak interfacial temperature decreased instead, owing to enhanced material extrusion and intensified heat dissipation. Meanwhile, the duration of the stable high-temperature plateau was markedly shortened. The corresponding experimental scheme is presented in Table 3.
From the overall variation trend (Fig. 12), within the investigated rotational speed range (2500 to 4000 r/min), the interfacial temperature evolution of both dowel materials exhibited a consistent pattern over time. The welding process can be divided into three distinct stages: rapid heating, high-temperature stabilization, and cooling. At the initial stage of welding, increasing rotational speed enhances the relative sliding velocity between the dowel and the hole wall, resulting in a marked increase in frictional work per unit time and a rapid rise in interfacial temperature. Once the process enters the stable welding stage, heat generation at the interface gradually reaches a dynamic balance with heat conduction and dissipation, and the welding temperature remains at a relatively high level. After welding is completed, rotation ceases and the interfacial temperature rapidly decays.
Table 3. Experimental Design under Different Rotational Speeds
Fig. 12. Effects of different rotational speeds on welding temperature for (a) Scots pine and (b) birch dowels
For the Scots pine dowel (Fig. 12a), the maximum interfacial temperature exhibited a trend of first increasing and then decreasing with increasing rotational speed. When the rotational speed increased from 2500 to 3000 r/min, the interfacial temperature rose significantly, indicating that a higher rotational speed improves frictional heat generation efficiency. With a further increase to 3500 r/min, the welding temperature remained at a relatively high level, although the increment became less pronounced. However, when the rotational speed was further raised to 4000 r/min, the maximum interfacial temperature decreased. This phenomenon is mainly attributed to excessive rotational speed causing the interfacial material to be expelled rapidly from the welding zone, preventing the stable formation of a plasticized flow layer. Meanwhile, part of the frictional energy is dissipated in the form of mechanical losses, thereby reducing the effective heat generation capacity.
In contrast, the birch dowel (Fig. 12b) produced overall higher welding temperatures than the Scots pine dowel under the same rotational speeds, and its temperature response was more sensitive to changes in rotational speed. When the rotational speed increased from 2500 to 3000 and 3500 r/min, the interfacial temperature increased markedly, and a relatively stable high-temperature plateau was formed in the medium-to-high speed range. When the rotational speed was further increased to 4000 r/min, the welding temperature dropped significantly, with a greater decrease than that observed for the Scots pine dowel.
Effect of Feed Rate on Interfacial Temperature
Figure 13 illustrates the influence of different feed rates on the interfacial temperature evolution during rotary friction welding of Scots pine and birch dowels, with heat-treated Scots pine used as the base material.
The feed rate mainly affects the thermal behavior of the welding process by regulating the effective friction time at the welding interface and the residence time within the high-temperature region. Under an appropriate feed rate, the welding interface can remain within a relatively high temperature range for a longer duration, which promotes sufficient softening and flow of lignin and hemicellulose, thereby facilitating the formation of a continuous and compact welded zone. In contrast, when the feed rate is excessively high or excessively low, the high-temperature plateau stage is significantly shortened, and both the peak welding temperature and its stability are adversely affected. The corresponding experimental scheme is presented in Table 4.
Fig. 13. Effects of different feed rates on welding temperature for (a) Scots pine and (b) birch dowels
Table 4. Experimental Design under Different Feed Rates
From the overall trend, under different feed rate conditions, the interfacial temperature evolution of both dowel materials exhibited a typical three-stage pattern of “rapid heating–high-temperature stabilization–cooling”. At the initial stage of welding, intense friction occurred between the dowel and the hole wall under the combined effects of axial feeding and high-speed rotation, leading to a rapid rise in interfacial temperature. During the intermediate stage, frictional heat generation and thermal diffusion gradually reached a dynamic equilibrium, resulting in the formation of a high-temperature plateau. After welding was completed, the interfacial temperature decreased rapidly as both feeding and rotation ceased.
For the Scots pine dowel (Fig. 13a), the maximum interfacial temperature generally exhibited a gradual increasing trend with increasing feed rate. When the feed rate was increased from 10 mm/s to 20 to 25 mm/s, the interfacial temperature rose markedly and the high-temperature plateau became more stable. This indicates that at higher feed rates, the frictional contact intensity between the dowel and the hole wall per unit time is enhanced, which facilitates the rapid accumulation of frictional work and thereby improves the heat generation efficiency at the welding interface. Meanwhile, a higher feed rate contributes to maintaining a continuous supply of softened material within the welding zone, promoting the stable formation of the welded band. In contrast, the birch dowel (Fig. 13b) exhibited more pronounced temperature differences under different feed rates. As the feed rate increased from 10 to 25 mm/s, the interfacial temperature increased significantly, and a relatively high and stable temperature plateau was formed at 20 to 25 mm/s. However, at a lower feed rate (10 mm/s), the interfacial temperature was considerably lower and the duration of high-temperature retention was shortened.
SEM Observation and Analysis of the Welded Zone Microstructure
SEM observations enable clear characterization of the entanglement and interlocking features within the welded zone. At a magnification corresponding to a scale of 10.0 µm, it can be distinctly observed that, after welding, the molten wood constituents underwent re-solidification and re-polymerization, becoming intertwined to form a continuous welded interface. This welded zone tightly bonded the dowel to the base material, thereby providing mechanical strength to the welded joint.
SEM images of welded specimens produced using the two different dowel materials are presented in Fig. 14. The welded zones are indicated by arrows, and the quality of the welded band can be clearly distinguished from the micrographs. These observations confirm that the wood cell-wall components softened and flowed during welding, and subsequently formed a densely interwoven structure upon cooling.
Fig. 14. Microstructural morphology of the welded zone after wood rotary friction welding. SEM images of the (a) Scots pine and (b) birch dowels; Arrows indicate welded zones