Interior wood coatings are routinely viewed at close range and encountered by homeowners and employees, making their appearance, durability, and potential effects on indoor health especially important. Many of the wood surfaces in indoor spaces are protected by clear coats, thereby revealing the wood grain patterns. This article reviews published information about interior wood coatings, with emphasis on appearance, health aspects, and protection of the wood. The stability of the color of indoor wood, especially with unpigmented coatings, can be affected by aging, by ultraviolet light coming through windows, and by unintentional spills. Limited ventilation of some interior environments provides a motivation to decrease reliance on volatile organic components of wood coatings, especially during their application. The literature reveals research progress in topics ranging from color and gloss, to durability, and to the minimization of adverse environmental impacts when coatings are used on wood surfaces that are exposed within houses and commercial buildings.


Download PDF

Full Article

Interior Wood Coating: A Review Focusing on Appearance, Health Effects, and Wood Protection

Hui Li , Paul Frederik Laleicke , and Martin A. Hubbe

Interior wood coatings are routinely viewed at close range and encountered by homeowners and employees, making their appearance, durability, and potential effects on indoor health especially important. Many of the wood surfaces in indoor spaces are protected by clear coats, thereby revealing the wood grain patterns. This article reviews published information about interior wood coatings, with emphasis on appearance, health aspects, and protection of the wood. The stability of the color of indoor wood, especially with unpigmented coatings, can be affected by aging, by ultraviolet light coming through windows, and by unintentional spills. Limited ventilation of some interior environments provides a motivation to decrease reliance on volatile organic components of wood coatings, especially during their application. The literature reveals research progress in topics ranging from color and gloss, to durability, and to the minimization of adverse environmental impacts when coatings are used on wood surfaces that are exposed within houses and commercial buildings.

DOI: 10.15376/biores.21.4.Li

Keywords: Wood coatings; Varnish; Gloss; Clear coats; Scratch resistance; Hardness; Color; Grain pattern; Emissions; Environmental impact

Contact information: Department of Forest Biomaterials, College of Natural Resources, North Carolina State University, Campus Box 8005, Raleigh, NC 27605-8005, USA;

* Corresponding author: [email protected]

INTRODUCTION

Why Apply Finish to Interior Wood?

The focus of this review article is on the interior wood coating, which is defined as the coating of wood surfaces intended for interior applications. Examples include self-standing furniture, built-in cabinets, flooring, doors, windows, paneling, and trim pieces. The coatings of interest can include varnishes, oils, paints, and self-curing formulations, such as epoxy systems (Hubbe and Laleicke 2025). Since indoor wood is often observed up close by the human occupants, there can be a high priority placed on appearance aspects, which can include scratch-resistance, gloss, and options to increase the visibility of the grain patterns of wood surfaces (Cox 2003). Another purpose of applying a coating is to protect the wood (Allen 1984; Flexner 1994; Cox 2003; Dvorák et al. 2023; Laleicke and Hubbe 2025; Grull et al. 2025; Xie and Xing 2026). The hardness of coated wood surfaces can be a priority concern not only for flooring, but also for wood-based writing surfaces and tabletops. As will be described in this article, both the selection of the wood and the details of coating selection and application can be important in meeting such goals.

In addition to scratches, unintended liquid spills represent another ongoing threat to the integrity and appearance of indoor wood (Miklecic and Jirous-Rajkovic 2021). Even indoors, there can be a need to achieve a suitable combination of hydrophobic character and resistance to permeation of water through the coating to the wood. Depending on the type of spilled liquid, an unprotected wood surface may become stained. Ideally, the wood surface ought to be washable with soap and water to remove any unintentionally spilled matter (Allen 1984). Even if staining is not regarded as a problem, cycles of repeated wetting and subsequent drying of wood surfaces can be expected to induce checking (patterns of cracks with repeated parallel or rectangular characteristics) of the wood surface (de Meijer and Nienhuis 2009; Gupta et al. 2015) or even cupping (Flexner 1994) due to uneven shrinkage. Such issues have been covered in greater detail in an earlier review article emphasizing outdoor applications of wood coatings (Laleicke and Hubbe 2025).

Because indoor conditions tend to be much less harsh, in terms of their effects on wood, in comparison to outdoor applications, there is much greater usage of clear coats (Evans et al. 2015; Torcatoru and Timar 2024). There is also more usage of optically transparent or translucent stains (Allen 1984; Landry and Blanchet 2012a; Landry et al. 2013). For this reason, this article will place emphasis on relevant issues in color and gloss measurements, as well as related factors in coating formulation to address appearance issues.

Challenges for Indoor Finishing

Indoor spaces raise concerns about formaldehyde, volatile organic compounds (VOCs), semi-volatile organic compounds (SVOCs), airborne particulates, and particles released as coatings wear or age (Flexner 1994; Howard et al. 1998; McCrillis et al. 1999; Kim 2010; Sherzad and Jung 2022). Abrasion and deterioration of polymeric films may contribute microplastic-sized particles, although evidence specific to aged interior wood coatings remains limited. Restricted ventilation can make indoor formulation and application constraints more demanding than those for exterior work (Laleicke and Hubbe 2025).

Though concerns related to ultraviolet (UV) light tend to be much reduced in comparison to outdoor wood applications, there can be specific concerns when a strong UV component of light enters by way of windows (Hundhausen et al. 2020; Vidholdová and Slabejová 2021; Slabejová et al. 2023; Torcatoru and Timar 2024). Since such UV exposure usually will not be accompanied by cyclic wetting and drying, it will not be classed as “weathering.” However, it still can induce color changes that fall into the category of “aging” (Vidholdová and Slabejová 2021; Torcatoru and Timar 2024). Figure 1 represents the case of a clear-coated wooden chair, as well as a varnished window frame, being subject to beams from the sun, shining through a window.

Schematic example of coated indoor wood exposed to sunlight; actual discoloration depends on wood species, coating, spectrum, intensity, and exposure duration.

Fig. 1. Schematic example of coated indoor wood exposed to sunlight; actual discoloration depends on wood species, coating, spectrum, intensity, and exposure duration.

Designers, interior decorators, furniture technologists, and householders face a wide range of choices, especially when it comes to suitable clear coats for indoor applications. The available classes of chemistry were described in more detail in an earlier review article (Hubbe and Laleicke 2025). Some points worth emphasizing in the context of coating of interior wood are listed in Table 1. Figure 2 shows key chemical structures of some of these options.

Recent developments in wood coatings include UV-LED and excimer curing, increased use of bio-based formulations, low-emission reactive systems, functional nanomaterials, and in-line process monitoring (Landry et al. 2015; Montazeri and Eckelman 2018; Halstensen et al. 2021; Song et al. 2024; Zhang et al. 2024c; Etxeberria et al. 2025). These approaches may improve curing efficiency, coating performance, production consistency, or environmental performance. However, spectral compatibility, cure depth, feedstock variability, long-term durability, equipment and implementation costs, industrial calibration, and verification of health and life-cycle benefits remain important limitations.

Table 1. Types of Wood Coatings and Some Key Attributes *

Types of Wood Coatings and Some Key Attributes

Types of Wood Coatings and Some Key Attributes

Basic chemical structures of resins in some widely used wood coatings

Fig. 2. Basic chemical structures of resins in some widely used wood coatings

Likewise, Fig. 3 shows the basic chemistry of a typical ultraviolet (UV)-curing type resin system used in wood coatings.

Structures of two typical UV-curing resins used in wood coatings and representation of their curing reaction

Fig. 3. Structures of two typical UV-curing resins used in wood coatings and representation of their curing reaction

Sources of Information

Two main types of input have been drawn upon by the authors in putting together this review article. On the one hand, aspects of wood coating technology that can be regarded as “best practices” have been established as a result of years of experience (Waring 1963; Allen 1984; Tichy 1997; Cox 2003). Thus, Allen (1984) encouraged readers of his handbook on wood finishing to envision themselves as “learning a craft”. On the other hand, ongoing research continues to reveal new options and a refinement in understanding of various mechanisms. For the latter input, the authors of this work have relied on research articles and US patents. Literature searching was carried out using the Web of Science database. However, as has been noted by Flexner (2005), it can be difficult to bridge the gap between practical experiences and scientific findings. The cited author found that he was able to succeed, at least to some extent, by asking a lot of questions of knowledgeable professionals, as well as by focusing on mechanistic aspects.

Previous reviews (Table 2) have generally emphasized exterior finishing, individual coating chemistries, or specific performance attributes. The present review addresses a remaining need by integrating appearance, human-health considerations, wood protection, application variables, sustainability, and coating mechanisms specifically for interior wood products. It draws on established practical guidance, recent research articles, and patents, and highlights agreements, chemistry-specific differences, recurring trade-offs, and unresolved questions.

Table 2. Review Articles and Textbooks Dealing with Aspects of Interior Wood Coating

Review Articles and Textbooks Dealing with Aspects of Interior Wood Coating

FACTORS AFFECTING INDOOR WOOD COATING PERFORMANCE

The subsections that follow have been arranged mainly in order of a typical overall process, though it should be expected that many variations in process order are possible. Some important factors include wood type, surface preparation (e.g., sanding), coating formulation and application, immediate and long-term protection of the wood, appearance, human comfort, and cost.

Wood Type

Wood selection affects both coating application and final performance. Density and hardness influence indentation support and abrasion response, while porosity and anatomical structure affect penetration and film uniformity. Lignin contributes to light-induced color change, and extractives can alter color, wetting, cure, and interfacial adhesion. For opaque trim paints, wood choice may be driven mainly by cost, strength, and freedom from defects; for transparent finishes, grain and inherent color become central (Allen 1984; Flexner 1994; Cox 2003). Keskin and Tekin (2011) compared cellulosic, synthetic, polyurethane, waterborne, and acid-hardening varnishes on several species and found that abrasion resistance depended on both wood and coating system. Kudela et al. (2023) used solvent-based polyurethane lacquer on spruce and oak and observed greater color stability for coated oak. These results illustrate that species effects should not be generalized independently of coating chemistry.

In cases where indoor wood is to be coated with an opaque paint, as is common for trim wood, windows, and some doors, it is expected that the selection of wood type will be mainly driven by considerations such as cost, mechanical strength, and a suitably low frequency of knots or cracks, etc. Wood selection, in combination with coating issues, can become more important when transparent or translucent coatings or stains are to be used (Allen 1984; Flexner 1994; Cox 2003). For instance, there can be a priority to select a combination of staining and clear coating treatment that will “show off” any wood that has been selected based on its interesting or attractive grain pattern or its inherent color (Flexner 1994). In addition, fine-grained hardwood such as walnut had been found to be more resistant to abrasion in comparison to a soft variety, such as pine, even after application of a coating (Keskin and Tekin 2011). Notably, the same relationship also has been reported with respect to color stability (Kudela et al. 2023). The cited authors applied solvent-based polyurethane lacquer to spruce and oak wood surfaces intended for indoor use. The coated oak wood was found to be more color-stable, as indicated by a lower value of the ΔE coefficient, representing the overall color difference before and after aging with exposure to ultraviolet (UV) light. Figure 3 shows an example in which an urban elm trunk was converted by the first author of this article into fine furniture by a process that included cutting a radial section of the trunk, milling, sanding, and application of a clear finish.

Example of an elm wood trunk after its conversion into fine furniture

Fig. 3. Example of an elm wood trunk after its conversion into fine furniture

Preparation for Indoor Finish Application

Sanding

As was noted by Allen (1984), the sanding of wood, as a way to prepare it for a coating application, can be optimized in view of how a typical coating works. Sanding conditions should be selected for the intended product, wood species, target appearance, and coating system. Initial sanding should remove machining defects, followed by progressively finer abrasives that are replaced as needed (Allen 1984; Flexner 2005). It has also been recommended that the initial sanding be carried out with sufficient coarseness to remove the largest blemishes, such as line patterns left over from a preceding operation, such as planing (Flexner 2005). Then, making sure to replace the sandpaper with suitable frequency, it is recommended to use a pattern of increasingly fine sandpaper, but not exceeding what will actually contribute to post-coating smoothness. Figure 4 illustrates the principle that different coarseness of sandpaper can be expected to yield different levels of roughness on wood surfaces. For instance, a 220-grit sandpaper can be expected to be sufficiently fine such that the remaining roughness will not contribute to the roughness or disturb the glossiness of a varnish coating (Allen 1984). Landry and Blanchet (2012a) achieved the best coating adhesion when using a 180-grit sandpaper on yellow birch, for waterborne coatings. A coarser sandpaper choice led to poorer wettability of the wood, due to the presence of large open cavities at the wood surface. On the other hand, excessively smooth sanding of the wood can be expected to reduce adhesion durability of the coating without contributing to smoothness or gloss (Sögütlü et al. 2016). Slabejová et al. (2016) observed a significant advantage of sanding in the grain direction; such sanding achieved higher gloss results.

Representation of the relationship between sandpaper coarseness (as indicated by the grit numbers “160” and “220”) and the resulting smoothness of the wood surfaces

Fig. 4. Representation of the relationship between sandpaper coarseness (as indicated by the grit numbers “160” and “220”) and the resulting smoothness of the wood surfaces

The foregoing discussion was based on an assumption that the sandpaper was sufficiently fresh, or in any case that debris has been periodically removed by slapping it against a hard surface. Excessive filling of sandpaper can lead to effects such as the smearing of greasy substances over the sanded wood surface, and it has been shown that such loosely attached compounds may not provide a firm support for the coating (Stehr and Johansson 2000). Likewise, wood particles transferred back onto the wood surface, especially if they are relatively large, may interfere with the smoothness of coated layers. A third likely consequence of the filling of sandpaper is a covering up of the abrasive particles, such that the sanding motions become ineffective in removing material from the wood surface.

Bekhta et al. (2022a,b,c) recommended gentle sanding between layers of interior wood finish, especially if there is concern about adhesion of the layers. Regarding the initial sanding, however, the cited authors evaluated an innovative approach – the substituting of thermal compression in place of sanding. Densification of the wood surface at 210 °C was found to provide suitable smoothness and improved color stability under indoor UV and infrared exposure, thus eliminating a relatively laborious and time-consuming sanding operation. Industrial adoption of this technique, however, depends on capital cost, energy demand, throughput, dimensional control, scale-up, and compatibility with the wood species and finish. Direct economic and life-cycle comparisons with conventional sanding remain limited.

In addition to sanding, several recently investigated methods can be used to modify the wood surface before coating. Atmospheric-pressure plasma can remove or oxidize hydrophobic surface components and increase surface energy, thereby improving the wetting and adhesion of waterborne coatings. Riedl et al. (2014), for instance, reported increased coating adhesion on plasma-treated sugar maple and black spruce, although the results depended on the wood species, plasma gas, and treatment time. Laser treatment also can clean or texture the wood surface, but its effect on coating adhesion depends on the treatment conditions, and excessive treatment may cause thermal degradation or discoloration (Kúdela et al. 2021). Gaseous ozone treatment provides another possible means of increasing surface polarity and wettability (Korpela et al. 2026). These methods appear promising for difficult-to-wet substrates and automated finishing operations, but they are not yet as widely established as sanding and primer application. While efforts to increase the wettability of surfaces before coating can be expected to improve the results for waterborne coating formulations, solvent-based coating formulations are less likely to need such treatments. Other work has shown that oil-based liquids spread readily on a wide range of surfaces, especially if those surfaces are initially dry (Hubbe et al. 2013; El Messiry and Fadel 2020; Liang et al. 2023).

Prime coats for clear finishes

After sufficient removal of any loose debris resulting from sanding, the recommended next step can be to apply a prime coat. As discussed in an earlier review (Hubbe and Laleicke 2025), the key purpose of such a coating is to achieve a strong bonding with the wood. This approach is based on an assumption that the interface between the coating and the wood will be the most likely point of the peeling of paint or other coating, if that were to occur in the future. To achieve relatively deep penetration of the primer coat into pores at the wood surface (e.g. vessels, tracheid lumens, ray cell lumens, etc.), primer coating formulations are prepared with relatively low viscosity. The moisture content of the wood at the time of coating also can affect the development of adhesion. Sönmez et al. (2009) found that varnish adhesion varied with wood moisture content, although the effect also depended on the wood species and type of varnish. Factors that favor good adhesion between successive layers of coating include application of the next coat within the recommended recoat interval, compatibility between the coating layers, and good wettability of the applied formulation onto a clean preceding layer. The recommended interval can vary greatly depending on the coating chemistry and curing mechanism. In addition, suitable porosity of the primer surface can promote mechanical interlocking, whereas reactive functional groups can provide sites for covalent bonding with the topcoat. If the preceding layer has fully cured or aged beyond the recommended recoat interval, cleaning and light sanding may be needed to improve inter-coat adhesion. Primer chemistry, porosity, degree of cure, and surface energy can consequently influence the wetting, spreading, and adhesion of the subsequent topcoat. These primer characteristics can also affect topcoat uniformity and the ultimate performance of the multilayer coating system.

A further motivation to apply a primer coat can be as a means to overcome problems with wood resins, such as tannins and turpentine components. Such compounds may migrate through layers of coating and discolor the coated wood (Bazin et al. 2026). It has been found that inclusion of a cationic resin within the primer formulation can be effective in preventing such exuding of wood resins into the finish layers of wood coatings (Bazin et al. 2026; Wu et al. 2026). Lu (2018) patented the use of a primer formulated with crosslinked polyvinyl acetate to seal wood surfaces to prevent leaching of wood preservatives. The patent by Wu et al. (2026) claimed the further inclusion of a polyisocyanate within such a primer formulation to improve sandability.

Whether or not a primer coat is justified will depend on the nature of the layers to be applied next, i.e. the finish coats or topcoats. Certain topcoats, both pigmented and clear, are formulated with the intention of achieving a smooth film, thereby providing a glossy appearance. The higher viscosity of such formulations makes them less effective in permeating into the surface pores of the wood. Peeling may develop in the future if such formulations are applied as the first layer onto wood, followed by the effects of time and usage. Figure 5 represents a hypothetical case in which a prime coat was apparently needed, due to the fact that the topcoat failed to achieve intimate contact with the valleys of roughness at the wood surface.

Schematic illustration of the importance of using a prime coat, which is designed to have a sufficiently low viscosity that it can achieve pervasive contact with the wood, deep into the valleys of roughness

Fig. 5. Schematic illustration of the importance of using a prime coat, which is designed to have a sufficiently low viscosity that it can achieve pervasive contact with the wood, deep into the valleys of roughness (e.g. lumens of tracheids and vessels), whereas certain finish coating formulations, which are designed to achieve surface quality, may have inadequate adhesion to the wood when used alone.

Coating Application Issues

When wood coatings are being applied by hand, an attentive person doing the work can be expected to be continually adapting their methods to achieve favorable coverage and an even appearance (Allen 1984; Flexner 2005). This optimization, based on watching the appearance of the wet coating surface, will depend on such issues as the viscosity of the formulation, the rate of evaporation, and a sense of whether there is suitably high wettability of the coating formulation on top of a preceding layer.

Viscosity

The viscosity of a coating formulation can have an important effect during its storage before use, during the application, and especially during the period right after application when the coating is still wet. For purposes of storage stability, there is a priority to minimize settling or creaming of coating components. That goal can be achieved by developing coating formulations having a plastic or pseudo-plastic rheological character (Kästner 2001; Larson et al. 2022). The binder or polymer itself is generally one of the largest contributors to the overall rheology of the coating. In waterborne coating systems, additional control of rheological behavior can be achieved by using associative thickeners, which are liquid rheology modifiers intended mainly for aqueous formulations (Larson et al. 2022). Such thickeners have a tendency to form transient structures among and between the components within the formulation, which can include the polymer (i.e. the thickener) and pigments (e.g. calcium carbonate or titanium dioxide), thereby tending to immobilize the formulation until stirring or another form of shear is applied. As an example, such behavior can be achieved by using a medium to high-mass acrylamide or acylate hydrophilic chain with an optimized substitution with short-chain alkyl groups. Transient self-association among such hydrophobic groups can be enough to prevent convective flow or settling within the mixture during storage or a few minutes after the mixture has been applied to the wood. There are further opportunities to achieve pseudoplastic behavior by incorporation of platy particulates, such as kaolin clays, sodium montmorillonite, or related products at sufficiently high levels to achieve transient “house-of-cards” structures (Okamoto et al. 2001; Wang and Pan 2025).

The viscosity and shear-thinning behavior also need to be matched to the coating application method (Eley 2019). Brush application generally requires sufficient low-shear viscosity to limit dripping while allowing the coating to flow and level under the shear generated by brushing. Roller application similarly requires a balance among coating transfer, resistance to splashing or sagging, and subsequent leveling. Spray application requires sufficiently low apparent viscosity under the high shear rates generated during atomization, although sprayability also depends on extensional rheology, coating solids, nozzle geometry, pressure, and equipment design (Elliott et al. 2007). Therefore, a universal viscosity range cannot be recommended; viscosity should be evaluated under application-relevant shear conditions and adjusted according to the coating formulation and application equipment.

Drying time to touch

Immediately after a coating layer has been applied by brush, roller, spraying, or other means, the layer will be vulnerable to events such as fingerprints, sagging, adhesion of dust, etc. (Dizman and Ozman 2020; Salata et al. 2020). To minimize such problems, some coating formulations have been optimized to relatively quickly develop a sufficient degree of curing, especially at the outer surface. The concept of skin formation is illustrated in Fig. 6, where the intensity of the red coloration is used to represent the progress of curing of the coating. Formulators of wood coatings need to optimize the speed of skin formation. Too rapid skin formation can lead to problems during application of the coatings. Too slow curing can lead to blemishes, such as when uncured coatings are touched too soon. A very slow cure may delay application of the next coating layer.

Concept of the progressive drying and curing of most types of wood coating, in which curing is associated with the evaporation of the fluid medium

Fig. 6. Concept of the progressive drying and curing of most types of wood coating, in which curing is associated with the evaporation of the fluid medium

Once a skin has been sufficiently developed at the freshly coated surface, it will no longer be tacky. In principle, this can be achieved by formulating at least one solvent (such as water or an organic solvent) that has a high enough evaporation rate, depending on the intended application (Hubbe and Laleicke 2025). In addition, the pseudo-plastic, self-associative nature of certain latex binder products can contribute to the immobilization of the freshly applied coating layer, such that it can tolerate gentle touching. In oxidative-drying alkyd systems, rosin-modified alkyd resins can be used to shorten the dry-to-touch time (Dizman and Ozman 2020). This approach is chemistry-specific and is not applicable to conventional waterborne latex coatings. Another widely used method, especially for factory-coated wood products, employs UV light to induce crosslinks for essentially full and rapid curing (Montazeri and Eckelman 2018; Hermann et al. 2021b).

Sanding between coats

Especially in the case of clear-coat layers for high-end interior finishing, e.g. for furniture, it has been recommended to gently sand between coating layers, using a relatively fine grit (Flexner 1994; Bekhta et al. 2022a,b,c). The purpose is not only to achieve a superior final smoothness, but also to achieve superior bonding between subsequent coating layers, especially in the case of topcoats that each have a smooth, glossy surface. Fine scratch-marks are expected to provide “tooth” and thereby enable good mechanical interlocking at the microscopic scale between the freshly applied resins and the previously applied solid layer (Hubbe and Laleicke 2025).

Time between coats

In most cases, a period of time between a few minutes and a few hours will be sufficient for most of the volatile components of a coating formulation to become fully evaporated (Flexner 2005; Wang 2022a,b). A dry appearance of the preceding layer can be used as initial evidence that sufficient time has passed that a subsequent layer can be successfully applied. The person applying the coatings also will be alert to whether or not additional drying time is needed for the solidification of material below a skin layer (Williams et al. 1996). For instance, the presence of liquid-like uncured formulation below a skin can become evident in cases where a stream of hot air is being used to accelerate curing of a wood coating, since the fully cured coating will not move or wrinkle upon application of the hot air stream. Too-fast drying of paint’s surface can be controlled with anti-skinning additives (Etxeberria et al. 2025). Environmental conditions also influence the appropriate interval between coats. Higher temperature and increased air movement generally accelerate evaporation, whereas high relative humidity can delay drying and film formation, particularly for waterborne coatings; excessive heating or airflow may promote premature surface skinning while the underlying material remains insufficiently cured (Keddie 1997; Song et al. 2023). Consequently, recoating decisions should consider the manufacturer’s specified temperature, relative-humidity, ventilation, and recoat-window requirements rather than surface dryness alone.

The above comments are likely to depend on whether or not the latest-applied formulation is waterborne or not. That is because the effective adhesion between the resins within successive coating layers is expected to depend on the activation of polymer segments in the resin components. The ideal goal would be to achieve mixing of between the respective polymers at the interface following application of the fresh layer (Deline et al. 1991). In general, such resins will be sufficiently hydrophobic that they will not be expected to swell appreciably when wetted by the water within a waterborne formulation. As a consequence, the two layers will fail to develop appreciable three-dimensional mixing at the interface. By contrast, an organic solvent in an oil-based coating formulation can be expected to swell and mobilize polymer segments (Li et al. 2026).

Immediate Physical Protection of the Wood

Especially in interior applications, people will have opportunities to look closely at coated wood surfaces. Damage, including scratches, indentations, flacking, or cracks in the finish, may detract from the ideal appearance (Cox 2003; Flexner 2005). Protection also will be needed against unplanned or occasional (e.g. due to washing) wetting by various liquids, including soapy solutions and food stains.

Scratch resistance

Scratch resistance can be defined, in practical terms, as the ability of a coated wood surface to resist changes in appearance in the course of ordinary rubbing against common household items, including clothing, cleaning devices, and items placed on the coated wood, etc. Scratches are most likely to result when hard particles or rough, hard objects are drawn across wood surfaces. Studies have shown that the scratch-resistance of wood surfaces can be enhanced by the applications of coatings. Such findings are highlighted in Table 3. Almost all of the cited studies have indicated positive effects. The protective effects generally can be attributed to the ability of resins within the formulation to fill in the voids of the wood surface, thereby achieving a denser and more continuous combined microstructure at the wood surface. Notably, scratch resistance depends on a balance between hardness and ductility rather than softness alone. In UV-cured acrylate systems, a ductile coating can accommodate deformation and limit brittle cracking, whereas a harder surface better resists penetration. Performance also depends on film thickness and substrate support: thicker or multilayer coatings can distribute stress, while dense wood generally provides greater support than low-density or porous wood. Therefore, coating chemistry and thickness, as well as wood species, density, and surface preparation, should be considered when comparing scratch resistance (Hermann et al. 2020, 2021a, 2021b).

Table 3. Studies Reporting Effects of Coatings on the Resistance of Wood to Scratching and Abrasion

Studies Reporting Effects of Coatings on the Resistance of Wood to Scratching and Abrasion

Studies Reporting Effects of Coatings on the Resistance of Wood to Scratching and Abrasion

Hardness

Figure 7 shows the principle of operation of the widely used Shore Durometer method for determining the hardness of different materials. This test device uses a spring to push an indentor towards the flat surface of a material of interest. The device can be easily calibrated, first by making sure that the pointer (or digital output) reads zero when there is no specimen. A standard very hard surface is then used to calibrate a maximum value of 100. The depth of penetration into the test material (shown at the right of the figure) will determine the value shown on the dial. The shape of the indenter depicted in Fig. 7 represents the Shore A tester, which is intended for relative soft materials. The hardness of the coated wood is often evaluated using a Shore D device, which is designed for harder materials and employs both a sharper indenter and a higher spring force than the Shore A device.

Principle of operation of the Shore Durometer test for hardness, where the intermediate range (Shore A hardness) is represented

Fig. 7. Principle of operation of the Shore Durometer test for hardness, where the intermediate range (Shore A hardness) is represented

In principle, there could be basically three ways to achieve increased hardness in wood coating, beyond what would have been achieved with a default formulation. As a primary consideration, the binder should be selected to have a suitably high glass-transition temperature, since this generally increases stiffness and resistance to indentation at the intended service temperature. However, an excessively high glass-transition temperature may interfere with film formation or reduce coating flexibility. In theory, the first would be to select a resin that tends to develop higher crystallinity upon evaporative setting of the coating. A search of the literature failed to find any example of such a strategy being used for formulation of a wood coating. A possible reason is that extensive crystallization might tend to render the material too brittle to perform its role successfully. A second approach relies upon cross-linking, i.e. chemical reactions resulting in covalent bonding between and among adjacent segments of resin (Czachor-Jadacka et al. 2021; Rosu et al. 2021). A prime example is the UV-cured coatings, which are popular for factory-finished furniture items (Landry et al. 2015; Hermann et al. 2021b; Mahajan et al. 2023). More recently, there has been increasing interest in the use of UV-LED systems for curing wood coatings. Such systems can provide rapid curing with relatively low heat generation and potentially lower energy usage. Successful application requires suitable matching between the emission wavelength of the LED source and the absorption characteristics of the photoinitiator, as well as sufficient penetration of the radiation through the coating layer (Landry et al. 2015). Thirdly, coating hardness can be achieved by optimized incorporation of hard mineral particles, under the requirement that there needs to be good wetting interactions between the mineral surfaces and the resins that are being used (Drelich and Miller 1995). In addition, hardness can be enhanced by the filling of pores in the wood surface, thus helping to resist indentation (Broda et al. 2023; Akbari et al. 2025).

In practical terms, the required hardness will depend on the intended use of the coated wood product. Flooring, stair components, and tabletops generally require relatively high resistance to indentation and wear, whereas appearance and flexibility may receive greater emphasis for cabinets, wall panels, and decorative furniture. It is also important to keep in mind that the measured hardness represents the combined response of the coating and the wood beneath it. Thus, coating chemistry, degree of cross-linking, and film thickness can interact with wood density, porosity, moisture content, and grain structure. A dense wood generally provides greater support to the coating, whereas a low-density or porous wood may deform under an applied load even when a relatively hard coating is present (Sönmez et al. 2011a,b; Hermann et al. 2021b; Kiliç and Sögütlü 2022a,b).

Highlights of articles dealing with hardness effects of wood coating formulations are presented in Table 4.

Table 4. Studies Considering Factors Affecting the Hardness of Coated Wood Surfaces

Studies Considering Factors Affecting the Hardness of Coated Wood Surfaces

Studies Considering Factors Affecting the Hardness of Coated Wood Surfaces

Resistance to flaking and cracking

Wood coatings may tend to peel, crack, or form flakes as they age, which can be attributed to gradual embrittlement and possible effects of moisture in the wood (Allen 1984). Contributing factors can include an excessively high glass-transition temperature of the binder, high volumetric contraction during curing, and inadequate adhesion between the coating and wood substrate. A high glass-transition temperature can decrease the ability of the coating to accommodate wood movement, whereas curing contraction can generate internal stresses within the coating layer. When resistance to the flaking or cracking of a coating is a high priority, some of the developmental strategies can be almost the opposite of these employed to develop hardness. For instance, both crystallization and cross-linking will tend to make the coating material less extensible, which can contribute to a brittle nature (Ansari et al. 2016; Kwon et al. 2024). Selection of resins that cure as an amorphous phase is likely to give a more extensible structure, which will be tougher and less likely to form cracks or flakes. Often a more practical way to increase the extensibility of a polymer-based material is to formulate it with a plasticizer, i.e. a monomeric or oligomeric substance that is highly compatible with the main resin but not having a tendency to form crystals (Gutierrezrocca and McGinity 1994).

Kiliç and Sögütlü (2022b) considered factors affecting the strength of adhesion of varnish to oak, chestnut, and pine woods. The strongest adhesion was with oil-based polyurethane varnish, which was followed by oil-based acrylic varnish, and then a waterborne varnish. Natural aging of the wood did not have major effects on the adhesion. Such adhesion is important because separation at the coating-wood interface can promote peeling or flaking even when the coating itself has adequate flexibility.

It is important to recognize that some of the properties just discussed can require trade-offs by the formulators of wood coatings. For instance, a primary goal to develop high resistance to flaking and cracking might lead to coatings having insufficient hardness. An excessively soft coating may also be susceptible to scratching. Sheng et al. (2021) reported an innovative way to overcome such issues by hardening the outside of an inherently flexible waterborne coating on wood. A polyurethane-urea coating on wood was hardened by treatment with zine carbonyl and zinc diamide pyridine compounds. The resulting coatings were found to be resistant to scratching.

Moisture barrier

Development of moisture barrier performance in wood coatings was considered in greater depth in an earlier review article focused on exterior wood applications (Laleicke et al. 2025). It is important to distinguish between resistance to liquid water and resistance to water vapor, since the mechanisms of transport are different. Indoor applications in which protection against liquid water will be important include table-tops, wooden floors (especially in kitchens and bathroom), and cabinets encompassing sinks and faucets. Such protection can be increased by selection of a more hydrophobic resin or by adding such components as wax to the formulation (Wang et al. 2025; Verduyn et al. 2026). Resistance to water vapor, by contrast, depends on the permeability, continuity, thickness, and degree of curing of the coating film. Thus, a coating that repels liquid water does not necessarily provide an effective barrier against water vapor. Miklecic and Jirous-Rajkovic (2021) demonstrated this distinction by showing that penetrating coatings protected wood against liquid water, but they were not effective against the effects of water vapor. Complete resistance to water vapor usually is not desirable for wood coatings. Rather, there needs to be sufficient water vapor permeability to allow gradual escape of liquid water, for instance in the case of accidental wetting of the wood due to spills or flooding.

Long-term Protection of the Wood

When the goal is to achieve long-term protection of interior wood, attention has to be paid to the durability of the coating material itself, as well as to the main degradative factors present during service. These factors include ultraviolet light entering through windows, changes in moisture content and relative humidity, exposure to heat, fire risk, mechanical wear, and effects of time. Aktas and Bilec (2012) demonstrated that the service life of indoor wood products can be predicted with satisfactory reliability based on an ASTM protocol and factor analysis. Social factors were found to have an important bearing on the results. A trade-off often needs to be reached between the cost of the initial coating and the time that passes before refinishing is recommended.

The relative importance of these factors depends on the intended use and location of the wood product. Moisture and changes in humidity can result in swelling, shrinkage, or loss of coating adhesion, whereas heat can accelerate coating and wood degradation. Fire-retardant performance also can be important for products used in buildings. UV exposure is of particular concern for surfaces receiving sunlight because it can cause changes in color and degradation of both the wood surface and the coating. The following discussion therefore considers these degradative factors and the corresponding approaches to protection.

The reason that ultraviolet (UV) light is a big concern, relative to the durability of wood, is that UV rays have sufficient energy to facilitate the decomposition of lignin (Moorhead and Callaghan 1994). The aromatic structures that compose lignin strongly absorb UV light, especially at wavelengths near 280 nm (Ruwoldt et al. 2022). Figure 8 shows four such structures that are common in natural lignin, and it also shows the corresponding wavelengths of maximum absorbance. When a photon of UV light is absorbed, an electron in the outer molecular orbital can be moved to an anti-bonding orbital, which may serve as a transition state in a potential breakdown pathway (Thomas et al. 1999). The further degradation of the lignin during interior exposure is expected to be quite different from exterior exposure, since it will not involve periodic rainfall, which would have removed the byproducts of lignin degradation (Laleicke and Hubbe 2025). Rather, such byproducts will be expected to remain in place, but in a modified and weakened form relative to the initial lignin.

Common functional groups within lignin that absorb ultraviolet light in the wavelength regions shown

Fig. 8. Common functional groups within lignin that absorb ultraviolet light in the wavelength regions shown (see Ruwoldt et al. 2022)

Ultraviolet light protection

For most interior wood products, exposure to UV light is less severe than for exterior wood because the building envelope and window glass reduce the amount of UV radiation reaching the surface. Nevertheless, prolonged sunlight through windows can cause discoloration and gradual degradation of exposed wood and clear coatings. The relative importance of UV exposure therefore depends on the location of the product; for surfaces receiving little sunlight, changes in humidity, heat, mechanical wear, and aging may be more important durability factors.

In cases where protection against UV rays is desired, there is a mature technology based on incorporation of substances having a strong ability to absorb UV light. These additives were discussed in an earlier review article (Laleicke and Hubbe 2025), and some highlights will be mentioned here. Titanium dioxide (TiO2) can be regarded as a benchmark against which the UV-absorbing materials can be judged. When the objective is to achieve UV production in a clear coat, the TiO2 particles should be about 50 nm or smaller, thereby avoiding strong scattering of visible light (Khanna et al. 2007; Qian et al. 2011). Premium TiO2 products for such purposes will have been prepared with a thin SiO2 coating on each particle, thereby avoiding adverse effects related to a tendency of the TiO2 to catalyze the formation of free radical species following the adsorption of photons of UV light (Veronovski et al. 2013).

Alternative materials for UV absorption include ZnO, CeO2, and various organic materials (Evans et al. 2015). Although lignin itself can be regarded as a UV-absorbing material, the ultimate goal is to avoid lignin breakdown in the underlying wood, below the coating. If follows that any lignin applied to wood as a UV absorber will likewise tend to become decomposed when exposed to a UV light source, such as near to a window, over a long stretch of time. Table 5 provides highlights from studies considering various additives to clear coatings to protect wood from the effects of UV light. Additional related studies were tabulated in an earlier review article that focused on outdoor applications of coatings, including clear coatings (Laleicke and Hubbe 2025).

Table 5. Studies Considering Additives to Protected Coated Wood from the Effects of UV Light

Studies Considering Additives to Protected Coated Wood from the Effects of UV Light

Tolerance to heating

In certain applications, such as a mantelpiece above a fireplace or a panel behind an interior heater, coated wood may be exposed to elevated temperatures. Such conditions can be expected to volatilize certain plasticizers and eventually to embrittle the polymers within coating layers. Atilgan and Sofuoglu (2023) showed that resistance to the effects of heating and thermal shock can be quantified by first heating to 50 °C for an hour and then abruptly switching to room temperature. Fifteen cycles of such treatment were found generally to decrease the gloss and increase the roughness of varnished pine, beech, and chestnut wood surfaces.

Fire resistance

Fire-resistant coatings have been widely studied, and examples are highlighted in Table 6. In principle, fire resistance can be achieved in three ways, which can also be combined. The three idealized mechanisms are illustrated schematically in Fig. 9. One way is based on formation of a sufficiently well integrated and thermally insulating char layer (Mensah et al. 2023; Liu and Fischer 2023). Another way is by absorption of heat, which is often associated with a phase change or dehydration reaction, resulting in the release of a gaseous byproduct (Shuyten et al. 1954). Thirdly, some initial resistance to fire can be achieved if released gaseous products, due to initial heating, are not flammable (Shuyten et al. 1954; Korobeinichev et al. 2022). Of these three contributions, the formation of a char layer has by far the most literature support and is expected to have the most durable effects, especially in cases where the wood material is thick.

Table 6. Studies Aimed at Achieving Fire Resistance by Means of Wood Coatings

Studies Aimed at Achieving Fire Resistance by Means of Wood Coatings

Illustration of three ways in which treatment of a coating formulation could be used as a way to decrease flame hazards

Fig. 9. Illustration of three ways in which treatment of a coating formulation could be used as a way to decrease flame hazards

Whenever substantial amounts of a specialized additive are used in formulation of a wood coating, potential adverse consequences need to be considered. In principle, addition of a flame-suppressing agent to such a formulation can be expected to dilute the effects of binders, thereby possibly weakening the resulting film. None of the articles cited in Table 6 evaluated such effects.

An issue that needs to be considered, with respect to fire hazards, is whether it might be unrealistic to rely just on changes to a coating layer, when the goal ultimately will involve the material as a whole. Thus, Sauerbier et al. (2020) reviewed related literature and recommended full impregnation of the wood as a preferred approach.

Appearance Effects of Clear Wood Coatings

The appearance of clear-coated wood can be affected by the clarity of the coating, by coloration, by gloss, and by other visual effects, including blemishes associated with the bleeding of wood resins from knots in the wood. Such issues have potential to decrease the value of the product.

Clarity

A key to achieving clarity in a wood coating, and thereby revealing the appearance of the underlying wood, is to minimize the scattering of light. One can envision a wood coating as being a form of composite, in which there can be different phases of material making up the film. High clarity requires either a minimization of differences in refractive indices of the phases that are present, e.g. a resin phase and a pigment phase (Sun et al. 2020) or keeping particle sizes much smaller than wavelengths of visible light (Veronovski et al. 2013; Miklecic et al. 2017). In addition, there must be no air gaps, micro-cracks, or bubbles within the coating, since air has a much lower refractive index than the other materials that make up wood coatings. As a demonstration of the importance of refractive index, it has been shown that transparent wood can be prepared by filling its voids with material that matches its refractive index (Wang et al. 2021; Chu et al. 2022).

Most binders and common pigments have refractive indices of about 1.5 to 1.6, which are highly contrasting with the value of 1.00 associated with air. Accordingly, a primary goal is that the coating ought to be free from both bubbles and crack-like void spaces. To minimize the likelihood of small air gaps between different materials within a coating, there needs to be good wettability among different phases (Kim et al. 2023). The same requirement is also important at the coating-wood interface (Hubbe et al. 2015), where the main concern will be on coating adhesion. When a coating has been prepared in such a way that there are no important transitions of refractive index within the layer, except in the case of particles much smaller than a wavelength of light, the result will be a high degree of transparency. Rays of light will tend to proceed through the layer as if it were a windowpane, without scattering or refraction. These relationships are illustrated schematically in Fig. 10, where it is assumed that the different phases have dimensions that are at least more than about 20% of the wavelength of light. Part A assumes equal refractive indices, as well as an absence of air gaps. Consequently, both the incident beam and the diffusely reflected beams from the wood surface are shown with no refraction (bending) or light scattering (partial dispersal of energy in other directions). Such expectations have been confirmed experimentally (Thorum et al. 2023). In fact, it is possible to produce nearly transparent wood material by impregnating it thoroughly with resin having a matched refractive index (Chen et al. 2022). As indicated in Part B, some light scattering is to be expected when a ray encounters a change in refractive index. In addition, the light will be bent like a prism if it strikes such a phase at a planar boundary other than a 90-degree angle (Guasti and Diamant 2012). The cited authors showed that the general relationship remains in effect, with moderate shifts in results, when there are gradual changes in refractive index rather than abrupt interfaces, e.g. when there is some mixing of polymer segments at an interface. The scattering of light, due to such circumstances, can be expected to decrease the clarity of the appearance of the underlying wood (Schmitt and Kumar 1998; Hendy 2002).

Illustration of rays of light passing through a coating with (a) well-matched refractive indices of different phases, and (b) different refractive indices

Fig. 10. Illustration of rays of light passing through a coating with (a) well-matched refractive indices of different phases, and (b) different refractive indices

Titanium dioxide particles, which are known as very effective absorbers of UV light, can be especially challenging due to their high refractive index. For particles having diameters more than a fraction of a wavelength of visible light (e.g. 100 nm or more), strong scattering of that light is expected, leading to an opaque film (Dietz 2023). However, many studies have shown that translucency can be achieved when yet smaller TiO2 particles are employed (Williams et al. 1996; Veronovski et al. 2013; Miklecic et al. 2017). Because of the high refractive index (2.55 to 2.7) of TiO2, the wavelength of light is temporarily decreased significantly as it passes through that phase. While such details are usually ignored, the practical effect is that formulators need to choose rather small nanoparticles, e.g. 25 nm (Veronovski et al. 2013), to achieve high clarity.

Boivin et al. (2019) considered the challenge of achieving resistance to black-stain fungal attack in the case of clear acrylic coating formulations. Silver nanoparticles were selected as the antifungal agent. Due to the small size of the particles, it was possible to maintain the translucency of the coatings. Particle-reinforced waterborne coatings of high clarity also have been prepared with cellulose nanocrystals (CNC), which have both nano size and a refractive index similar to that of resins used in wood coatings (Vardanyan et al. 2014, 2015; Yang et al. 2020; Khan et al. 2022). Landry et al. (2010) showed that incorporation of organically modified montmorillonite (nanoclay) particles into UV-curable wood coatings gradually increased the haze of the resulting cured coatings as the clay content was increased up to 10%. Taken together, these findings show that functional nanomaterials can be used to provide UV protection, antimicrobial activity, reinforcement, or controlled optical properties. Their successful use requires good dispersion and compatibility with the coating resin. Further attention also is needed with respect to transparency, long-term retention of performance, and possible release of the particles during usage, refinishing, or disposal.

Wood grain appearances have been studied with respect to their perception and emotional impact (Wan et al. 2021). Wood often has been described as having a calming effect, but people’s reactions to different grain patterns are highly varied (Song and Zhao 2011). Studies have shown that wood surfaces tend to be perceived as warm, regardless of their actual temperature (Zhang et al. 2024a, 2025). Studies have shown a positive effect of heat treatment on people’s perceptions, and this has been attributed to a reddening effect and more pronounced grain pattern (Zhang et al. 2024b). Certain woods are in demand due at least in part to their attractive annual ring patterns (Nakamura 2012). It has been reported that application of a clear coat can increase the visibility of the grain pattern (Tao et al. 2024). Swartz et al. (1999) claimed the use of a clear coating that was formulated to accentuate grain patterns in furniture or carved wood; this was achieved partly by enhancing red and yellow hues, while suppressing blue and gray. Gertzmann et al. (2017) claimed the use of a waterborne acrylic coating for rendering wood grain more visible.

Song et al. (2024) prepared lignin/titanium dioxide nanoparticulate composites, with the goal of achieving both UV protection of the wood and high visibility of the grain pattern of oak wood. The authors reported that the decorativeness of the wood was enhanced. In addition, the color remained unchanged after extensive exposure to UV light. Tao et al. (2024) showed that similar effects can be achieved by means of metallic particles as a coating component.

Gloss

Homeowners, designers of office spaces and furniture, and buyers of indoor wood items will have a wide range of preferences regarding glossiness. The preferred gloss level also will depend on the intended application. High-gloss coatings may be selected for decorative furniture when there is a desire to emphasize the wood grain, whereas satin or semi-gloss finishes are often preferred for flooring because they provide some sheen while making scratches and wear less noticeable. Matte or low-gloss coatings may be favored for wall panels and other large surfaces where there is a priority to minimize glare and the visibility of surface irregularities. Gloss can be quantified by measuring the ratio of reflected to incident light intensity of a specified wavelength or wavelengths at a specified angle (20°, 60°, or 85°) (Lindstrand 2005; Chadwick and Kentridge 2015; Kilic and Sögütlü 2020). A high degree of gloss may be desired, for instance, as a means of maximizing the clarity of wood grain patterns in attractive wood furniture. By specularly reflecting incident light, as well as taking advantage of humans’ innate tendency to avoid viewing objects at a glare angle, the light coming from the glossy coated wooden object is less diluted by diffusely reflected light from the wood surface (Cuppo et al. 2013; Hauptmann et al. 2013). This results in a stronger perceived contrast of light intensity from adjacent areas.

Figure 11 contrasts a glossy paint with a semi-gloss, and a matte coating, in terms of how each of them affects the specular reflection of light.

Schematic comparison of the relationship between surface smoothness, the extent of specular reflection from a coated surface, and the degree of sensation of gloss, semi-gloss, or matte effects

 

Fig. 11. Schematic comparison of the relationship between surface smoothness, the extent of specular reflection from a coated surface, and the degree of sensation of gloss, semi-gloss, or matte effects

To achieve a high level of gloss, the surface needs to be smooth down to the dimensions of the wavelengths of light. Semi-gloss and matte coatings, to be discussed later, exhibit either less or very little specular reflection. In the case of matte coating, the incident light is either diffusely reflected (i.e. scattered) or absorbed by chromophores in the coating.

High levels of gloss in coated wood can be achieved with a combination of careful workmanship and appropriate formulation of the coating. The workmanship will have already begun with the sanding procedures discussed earlier. Emphasis will be placed on selecting a suitably fine final grit level in the sanding sequence (e.g. in the range of 180 to 220 according to Allen (1984) and Flexner (2005)), such that the remaining roughness no longer has any effect on the final measured roughness. In general, that means that the roughness should be well below the intended average thickness of the coating layer.

Table 7. Highlights from Studies Considering the Gloss of Wood Coatings

Highlights from Studies Considering the Gloss of Wood Coatings

According to James and Taifa (2023), high gloss can be promoted by using a relatively low resin content in an alkyd coating formulation. Thickness should be reported as dry-film thickness and selected for the coating chemistry, solids content, number of coats, substrate, application method, manufacturer’s specification, and relevant performance standard, etc. Table 7 provides highlights from studies in which factors affecting the gloss of coated wood were studied.

Coating formulations need to be optimized to achieve a favorable balance between curing rate, rheological properties, and the fact that some time will be required for localized flow after the coating has been applied to the wood. An excessive rate of evaporation, coupled with too high viscosity, will mean that any wave patterns or brush marks produced during the application may remain after the coating has dried. In some cases, these features may become permanent as soon as a skin has formed at the surface of the freshly applied coating. Formulators often will aim for a compromise among different desirable outcomes, especially with respect to the setting time of coatings. Thus, it can be advantageous for the coating to become quite quickly immobilized and thereby somewhat resistant to sagging, fingerprints, and the permanent adhesion of dust. In some high-end coating operations, intended for superior gloss, there can be a preference for slower-drying formulations, and therefore steps are taken to ensure a dust-free air environment (Cox 2003).

Matte effects

When formulators of wood coatings want to achieve a “matte” effect or a semi-gloss effect, the usual approach is to incorporate particles that are large relative to the wavelengths of visible light (Flexner 1994; Zhu et al. 2023). Fumed or precipitated silica particles are sometimes used for this purpose (Royall and Donald 2002). Such particles cause a fraction of the light striking the surface to become diffusely reflected in all directions (Wan et al. 2021). Such particles function as matting agents. During film formation and drying, they protrude slightly from the coating surface and produce microscopic surface roughness. The resulting surface texture scatters incident light in different directions and thereby decreases specular reflection. Thus, the matte appearance results mainly from the surface roughness produced by the matting agents, rather than from the particles merely being present within the coating film. As a consequence, colored coatings become less saturated, meaning that more white light becomes mixed with the light perceived by the viewer. The general change in appearance can be described as a softening effect. In the case of clear coatings, the underlying wood grain patterns will become less pronounced. Because the gloss-defeating particles function by scattering some of the light towards the viewer, the net effect may be an increase in the lightness value L*, in terms of the widely used CIE L*a*b* system (Hauptman et al. 2013; Wan et al. 2021).

Not all matte effects are achieved by means of particles. Excimer-matte technology uses short-wavelength, nearly monochromatic UV radiation, commonly at 172 or 222 nm, to cure only a very thin region at the coating surface. Contraction of this surface layer produces microscopic wrinkles that scatter light, after which a conventional UV source is generally used to complete curing through the coating thickness. This approach has been investigated since at least the late 2000s and has subsequently been adopted for factory-applied ultra-matte finishes on furniture and wood-based panels (Bauer et al. 2009; Cefla Finishing 2022). Zhang et al. (2024c) examined a related excimer-matte approach in which a polyurethane acrylate wood coating was irradiated by 222 nm far-UV radiation, as can be provided by an excimer lamp, giving rise to micro-wrinkles. The results were able to be controlled, to some extent, by varying the curing temperature, film thickness, and photoinitiator concentration. Such an approach offers a means of achieving a matte surface without relying entirely on the addition of particulate matting agents.

Coloration in clear coatings

Some of the most commonly used stain pigments, for use with clear-coated wood systems, are based on tannic acid, potassium permanganate, and iron compounds (Allen 1984). In the case of tannic acid, a darkening effect can be achieved by raising the pH, e.g. with ammonia or KOH (Kropat et al. 2020). Typical stain formulations are applied by diluting them and spreading them evenly onto uncoated wood (Allen 1984). Alternatively, the staining of challenging wood types such as pine and fir may prompt the worker to first apply a dilute sealant or “wash coat,” thereby reducing the amount of uptake of stain into the wood (Allen 1984; Flexner 2005).

In addition to benefitting from high clarity and transparency of the coating, annual ring patterns in wood can be rendered more visible by well-chosen applications of stains. In the case of pine wood, the lower-density earlywood layers within each ring tend to become more deeply stained than the latewood layers, which are denser (Flexner 2005). This tendency can reverse the original pattern, in which higher lignin content in the latewood may contribute to an initially darker appearance. In other cases, staining treatments have been optimized when there is a goal to decrease the contrast of wood grain patterns (Flexner 2005).

Another way to achieve staining effects is to add the pigment to a clear-coat formulation. For instance, Goktas et al. (2023a) added environmentally friendly colorants from purple cabbage, safflower, and beets to water-based lacquer formulations. The colorants appeared to be effective for indoor applications, at least during the period of testing. Follow-up tests (Goktas et al. 2023b) showed inadequate resistance to fading, based on 50 days of outdoor exposure. Because colorants perform their functions by absorbing light’s energy, some of them are vulnerable to fading. In particular, when the colorants are based on organic chemicals, the absorption of light, especially in the UV range, can yield transient unstable molecular structures that can lead to decomposition (Colombini et al. 2007).

Color changes of clear-coated wood upon UV exposure and aging

Color is commonly evaluated in CIELAB space using lightness L*, red–green coordinate a*, yellow–blue coordinate b*, and total color difference ΔE*. More specifically, an increase in a* indicates a shift toward red, whereas a decrease indicates a shift toward green. Likewise, an increase in b* indicates a shift toward yellow, whereas a decrease indicates a shift toward blue. A decrease in L* represents darkening, while an increase represents lightening (CIE 2018). Clear coating often initially darkens wood by reducing air-filled surface scattering; subsequent aging may decrease or increase L* and shift a* or b* depending on wood species, coating chemistry, stabilizers, and exposure. During simulated indoor light exposure, ΔE* generally increased with exposure time, but the changes in the individual coordinates depended on the wood species and coating system. For example, polyurethane-coated spruce generally showed decreasing L* and increasing a* and b*, whereas coated oak sometimes showed an initial decrease followed by a moderate increase in L*. Thus, coated wood may darken and yellow initially, but partial lightening can occur during continued exposure in some wood–coating combinations (Kúdela et al. 2023). Accordingly, no universal indoor-aging trajectory should be assumed. Much of the scientific literature concerned with the coloration of coated wood products has been focused on coloration of the wood itself, as well as changes to the coated wood color in response to ultraviolet light, as well as aging. Highlights of such research are summarized in Table 8. Note that none of these results reported here involve the application of both UV light and water, a combination that was considered in an earlier review dealing with outdoor wood coating (Laleicke and Hubbe 2025).

Table 8. Highlights from Studies Concerning the Color of Coated Interior Wood

Highlights from Studies Concerning the Color of Coated Interior Wood

Highlights from Studies Concerning the Color of Coated Interior Wood

The initial darkening effect reported by Mendes et al. (2016) is consistent with the principles of light scattering and absorption (Kubelka and Munk 1931; Yang and Kruse 2004). Lumen spaces and other pores having a size of about 0.2 μm or greater will scatter some of the incident light in all directions (diffuse scattering), thereby making the material appear lighter. When those same pores near to the wood surface become filled with clear material having a refractive index nearer to that of the wood material, such light scattering can be greatly reduced. According to Kubelka-Munk theory, light absorption effects tend to become more prominent when light scattering is reduced.

Pigments and Natural Colorants for Wood Coatings

Colorants to be used in opaque paint formulations require high durability, strong absorption of light, and predictable spectral characteristics. Though, in principle, it would be possible to formulate desired color effects for wood coatings with use of organic pigments, i.e. dyes, the resulting coatings would be expected to lack the needed light-fast character. For this reason, inorganic pigments are mainly used for such purposes as colored stains and opaque paints (Buxboam and Pfaff 2005). Four main classes of pigments used in paints are represented in Fig. 12.

Representations of the four main classes of opaque pigments that are widely used in wood coatings

Fig. 12. Representations of the four main classes of opaque pigments that are widely used in wood coatings

Metal oxides

Among the inorganic pigments, titanium dioxide (TiO2) has by far the greatest usage. Due to the very high refractive indices and light-scattering ability of the rutile and anatase mineral forms of TiO2, they have a dominant role in providing opacity, in addition to white coloration in commercial paints. Next in terms of usage amount are the iron oxides, which are especially used in red paints and stains. For example, red coloration can be provided by α-Fe2O3 (hematite). Because this is a highly stable crystalline mineral, it exhibits high resistance to fading. Iron oxide varieties are also widely used to achieve orange, yellow, brown, and even some blue colorations. Such effects are achieved not only by selecting different oxide forms, but also by optimizing the particle sizes. Chromium-containing pigments, such as Cr2O3, are used for green colors. Blends of this pigment with iron compounds are used for some greens and blues.

According to Buxbaum and Pfaff (2005), most commercially sold inorganic pigments are coated with oxides or hydroxides. Such treatment, in the case of TiO2, is carried out due to the photoactive nature of the pigment. Absorption of UV light by the TiO2 otherwise would give rise to free-radical species, which could become involved in the chemical breakdown of a coating or in a bleaching effect on any organic colorants. Other additives, such as surfactants and polymers, can be used to optimize the dispersion of the pigment slurry and its tendency to remain smooth and unagglomerated during storage.

Carbon black

Carbon black is the dominant black pigment and is conventionally produced from petroleum fractions by partial combustion (Buxbaum and Pfaff 2005). Biomass-derived biocarbon offers potential advantages through renewable feedstocks and waste utilization (Aprianti et al. 2023; Drupitha et al. 2023). Its use as a substitute requires control of particle size, color strength, surface chemistry, dispersion, purity, ash, batch consistency, process energy, and scale-up. Environmental advantage should therefore be established by performance-normalized life-cycle assessment rather than renewable origin alone.

Colorants from plant materials

In view of increasing public interest in use of natural organic materials, Fig. 13 represents two classes of colorants that can be obtained from plant materials and used for the darkening of wood. As shown in part A of the figure, natural tannins, especially when treated with a strong oxidizing agent, produce a dark pigment (Aguilar et al. 2007). Part B of the figure shows four lignin-derived functional groups that are known to absorb light strongly in the visible range (Gratzl 1985; Paulsson and Parkås 2012). The darkening effect due to such lignin functional groups often can be made more intense by treating the wood material with alkali (He et al. 2004).

Examples of widely used natural-derived chromophores that can be used to darken the appear-ance of wood, as in stains and as components of formulations for clear coatings: A. Oxidized tannins; B. Chromophoric groups associated with lignin

Fig. 13. Examples of widely used natural-derived chromophores that can be used to darken the appearance of wood, as in stains and as components of formulations for clear coatings: A. Oxidized tannins; B. Chromophoric groups associated with lignin

Special Optical Effects

Thermochromic effects

In addition to effects related to gloss, there are a wide range of other optical effects that have been considered at a research level. For example, thermochromic effects were reported by Yan et al. (2019), meaning that the color of the coated wood changed in response to temperature. Upon removing the heat source, the appearance changed back to the original. This was achieved by encapsulating the thermochromic dye in a paint base. As an example, by heating the coated wood to 32 °C, the coated wood was changed from yellow to colorless (Yan et al. 2021). Related work showed that such effects could be achieved with only minor effects on gloss and adhesion of the coating to the wood (Yan et al. 2020a).

Glitter effects

Glitter effects, when desired, can be achieved by application of flakes of reflective material, formulated in a clear mixture with resin and fluid medium. The glitter particles can be, for example, cut flakes of metal-coated plastic film (Tagg and do Sul 2019). Because such particles fall into the category of microplastics, and due to their widespread usage in cosmetics, there have been studies of their presence in the environment (Yurtsever 2019).

Structural iridescent and non-iridescent effects

Structural colors are responsible for some striking effects, such as the wings of butterflies (Kinoshita and Yoshioka 2005). Rather than relying on the absorption of light, the apparent colors are due to the precise spacing of tiny details, such as lines. Figure 14 illustrates two rudimentary examples.

Simple examples in which uniform structures, such as (A) thin films such as bubble walls, or (B) highly regular alternating layers of specified thickness and refractive index, can provide vivid color sensations without the use of any chromophoric substances

Fig. 14. Simple examples in which uniform structures, such as (A) thin films such as bubble walls, or (B) highly regular alternating layers of specified thickness and refractive index, can provide vivid color sensations without the use of any chromophoric substances

Table 9. Highlights from Studies Concerning Structural Colors in Films

Highlights from Studies Concerning Structural Colors in Films

With advancement of digital printing technology, it is now possible to achieve such effects on wooden surfaces. For instance, Sang et al. (2023a,b) evaluated different wood coating approaches to produce a suitable white background on wood, upon which to 3D-print high-quality images that can include structural color effects. Table 9 highlights findings from several studies that have considered the usage of structural color effects in coatings. Though only one of these examples (Yang et al. 2019) involved application to a wood surface, it appears that such technologies have wide tolerance for a variety of surfaces, which could include wood. There appears to be a rapid pace of technology development, leading to several competing ways to achieve non-fading, bright colors that in the future could be used in wood coatings.

Simulated weathering

Another class of modifications to wood surface falls under the category of “simulated weathering” of wood (Kropat et al. 2020). Though such modifications can span a very wide range of creative treatments, a common theme is that the resulting appearance needs to be markedly changed, and it needs to be attractive to at least some potential clients. For example, application of gray paint can convey, to some extent, an impression of oldness, as part of a decorative scheme for wood items (Hundhausen et al. 2020).

Retroreflective coatings and paints

Spherical glass beads, often having a diameter of about 200 to 500 µm, are widely used in highway line markings, roadway signage (Bible and Johnson 2002; Ivanov et al. 2006), and license plates, and they are more recently being considered for minimizing undesired solar heating of buildings (Levinson et al. 2020; Yuan et al. 2025). Such features become important at night when motorists have turned on their headlights. As illustrated in Fig. 15, light that strikes the so-called retro-reflective surfaces bounces off a reflective material on the back side of the bead and tends to return in the approximate direction from which it came, thus making certain features highly visible to the driver. To achieve such effects, some of the spheres need to be present at the coating surface, such that incident light is not obstructed by any pigments present in the coating. A light ray that enters into one of the spheres will tend to be reflected within the sphere in such a manner that it returns towards its source direction, thereby creating a glare-like effect. Though such coatings are most often applied either to steel surfaces or to pavement surfaces, they could, in principle, be applied to wood.

Principle of retroreflective spherical glass particles, which shine a beam back in the direction of an incident beam

Fig. 15. Principle of retroreflective spherical glass particles, which shine a beam back in the direction of an incident beam

Knot Bleeding Resistance

Unattractive splotching effects can happen in cases where there is seepage of wood resins into paint layers. Such effects are often attributable to the bleeding of monomeric compounds such as terpenes and tannic acid from knots in the wood (Allen 1984; Williams et al. 1996). It is inherently difficult to block such compounds from seeping into coating layers due to their mutual solubility with typical resin components in wood coatings, in addition to their low viscosities in some cases of greatest concern. Problems became especially notable as practitioners began to replace oil-based coatings with waterborne latex formulations (Kimerling and Bhatia 2004). Bleeding problems have been addressed in various ways, such as by applying a primer coat (Williams et al. 1996). In the case of high-end items, steps can be taken to extract monomeric oleophilic compounds from the wood, for instance by using oxalic acid and detergent (Williams et al. 1996). Published findings providing details about such issues are highlighted in Table 10.

Table 10. Highlights from Studies on the Show-through of Wood Resins through Paint Layers, Especially in the Case of Knots

Highlights from Studies on the Show-through of Wood Resins through Paint Lay-ers, Especially in the Case of Knots

Comfort

When a person touches a coated wood surface, there may be impressions of temperature, smoothness, or frictional effects that can influence the mood of an individual. The tendency of a coated wood surface to exchange heat with an applied hand or finger can be expected to depend on three factors, namely heat capacity, heat conductance of the wood, and the efficiency of heat exchange at the point of contact with a hand or finger.

Temperature effects – Phase-change materials

A high ability to store and release heat within selected temperature ranges has been achieved by the use of so-called phase-change systems (Sharma et al. 2009; Bai et al. 2022). When the melting and freezing take place at a comfortable temperature suitable for a dwelling or workplace, a phase-change material can contribute to maintaining temperatures in a desirable range with a net decrease in the energy that needs to be expended for heating or cooling. Bai et al. (2022) achieved such effects by placing phase-change material in microcapsules, which were then incorporated into the formulation of coatings for wooden furniture. The effects were verified by thermal measurements.

Temperature effects – Heat transfer from the hand

Heat conduction between a hand or finger and a coated wood surface will depend not only on thermal conductance of the materials, but also on the efficiency of contact – which is likely to involve microscopic air gaps due to roughness. Because wood can generally be classed as a thermally insulating material, humans generally perceive it as being “warm” (Zhang et al. 2024a,b), despite the fact that it is likely at room temperature (e.g. 25 °C in some air-conditioned offices), and the human body temperature (37 °C) will be about 12 °C warmer. When there is a goal to further reduce any feeling of coldness, the formulator of wood coatings can increase the roughness of the surface. In this way, the contact between the solid surface involves less area, and any possibility of a cold sensation is reduced.

In addition to genuine issues related to the transfer of heat, it has been shown that the appearance of coated wood surfaces can also affect people’s perception of warmth or coldness (Poirier et al. 2019; Zhang et al. 2024b, 2025). Based on their tactile experience, people will naturally anticipate that a surface having a wood-like appearance is unlikely to conduct a lot of heat away from a hand placed in contact with it. Smooth, glossy surfaces will tend to be perceived as having high contact efficiency with an applied hand; it follows that such surfaces will be expected by the human to feel cold (Zhang et al. 2025). Such results can depend on whether the observer is using their eyes, their fingers, or both (Zhang et al. 2025).

Tactile effects

When a person’s hand passes over a solid surface, the tactile impression will be affected by such attributes as smoothness, morphological patterns, and the coefficient of friction. As illustrated in Fig. 16, the human perception of surfaces can be understood as coming from a combination of sensations from the fingertips (surface perception) and other parts of the hand (for so-called bulk perception) (Wang et al. 2019).

Illustration of some ways in which the surface nature of wood can affect the perception of such attributes as softness, smoothness, slipperiness, or friction

Fig. 16. Illustration of some ways in which the surface nature of wood can affect the perception of such attributes as softness, smoothness, slipperiness, or friction

The bulk attributes are important, for instance, in the evaluation of the softness of tissue paper products, which can be crumpled in the hand. The surface perceptions are expected to take on a dominant role in the case of wood surfaces due to their general level of hardness. As illustrated in the figure, the perception of smoothness or softness is expected to depend not only on the degree of roughness, but also on the possible presence of any slippery or tacky substances on the surface. Loose particulate matter, especially talc or hard bead-like dust will impart a slick feel to the surface (Abdulkareem et al. 2010; Faiyad et al. 2025), though such effects are likely to be removed by washing with soap and water. By contrast, higher friction can be imparted to the surface by rubbing on a thin layer of rosin or similar materials (Smith and Woodhouse 2000). As noted in the cited article, rosin causes stick-slip behavior when a surface, such as a violin string, is being rubbed.

Ramanakoto et al. (2017) studied factors affecting consumer preferences in the case of machined wood surfaces. It was found that consumers placed emphasis on their tactile sensing and that they appreciated smooth surfaces of furniture items. The tactile information acquired by the panelists was supplemented by their visual observations of such features as defects and waviness of the surface.

In principle, the coefficient of friction of a coated wood surface can be adjusted by selective use and levels of certain additives. For example, wax is a common additive in wood coatings or impregnation (Wasserman and Ahmed 2024), and it inherently provides a slippery feel.

Among the various engineered wood products available on the market are particleboard panels to which faux wood grain patterns have been applied in the course of hot-pressing. These patterns can be perceived both visually and by feel. Rather than hiding an underlying grain pattern, an opaque coating on such a particleboard surface helps to hide the fact that the underlying grain pattern is not real. Nevertheless, the wood-like patterns of ridges and valleys may convey a sense of wood-based origin, whether or not the annual ring patterns are genuine. Akiyama et al. (2014) reported that a more convincing computer-generated pattern of wood grain can be achieved by incorporating information about tree growth and the resulting anatomy into the computer program. Gaff and Gasparik (2013) and Gaff et al. (2017) studied factors related to the production of high-quality embossed patterns on aspen wood.

Costs of Coating Applications

Labor remains a major cost in interior wood finishing (Kardar and Amini 2024). In factory finishing operations, however, increasing use is being made of automated mixing and dispensing, robotic spray application, UV or UV-LED curing, in-line sensing, and digital process control (Landry et al. 2015; Arrais et al. 2021; Halstensen et al. 2021; Xu et al. 2024). Such technologies can contribute to improved transfer efficiency, more consistent coating application, increased production rates, and earlier detection of surface defects. On the other hand, these potential benefits need to be balanced against the costs of equipment, maintenance, programming, worker training, and the need for a sufficient volume of production. Thus, the economic justification for automation will depend on the scale of operation and the variety of products being finished.

Studies have shown that multiple layers of wood coating often can achieve not only better coverage but also higher durability (Hysek et al. 2018; Grüll et al. 2014; Laleicke and Hubbe 2025). Each applied layer will add to the labor costs and also to the time needed to complete the job. In manually applied finishing operations, the worker will be able to sense whether an excessively thick coating layer, as a strategy to skip a step, is interfering with their goals of achieving uniform coverage and smoothness with each coat, while avoiding teardrop effects on vertical surfaces or wet spots on horizontal surfaces (Larson et al. 2022). With such considerations in mind, there is a high priority to use a coating formulation that is well-suited for each job, rather than just achieving a low labor cost.

ECO-FRIENDLINESS AND HEALTH

Health and environmental aspects of wood coatings are receiving increasing attention (Nakanishi et al. 2024). Interior coatings receive particular scrutiny in this regard, due to issues as limited ventilation in some indoor settings (Sherzad and Jung 2022; Main et al. 2024). Also, there is a trend toward increased time that people spend indoors on average (Brasche and Bischof 2005). The study by Mai et al. (2024) revealed that application of wood coatings during the renovation of existing houses can be especially hazardous due to high releases of known and unknown compounds and the fact that people may be present in the building either during the project or soon thereafter. People’s proximity to the surfaces of indoor wood can increase their exposure to volatile organic compounds (VOCs) and other airborne contaminants associated with wood coating. This section will consider the release of volatile substances both during the application of a coating and later. It will consider coating systems based on the idea of sealing an engineered wood surface to slow down the escape of such compounds as formaldehyde (Boehme 1995; Kim 2010; Ding et al. 2013; Salthammer 2019). In particular, the review article by Salthammer (2019) reported that coatings of various types have been able to drastically decrease formaldehyde releases within houses, presumably by blocking the passage of such compounds from the underlying engineered wood materials. Finally, it will consider the importance of wood durability, as a means to minimize environmental impacts by postponing the need for items or housing to be replaced or refinished.

Fumes While Applying Finish

As already noted, the greatest release of volatile organic compounds from wood coatings can be expected during their application (Mai et al. 2024). Associated risks can be mitigated by isolation and ventilation, especially in the case of factory-finished items. These are often coated with conversion coatings, which tend to emit high levels of VOCs and formaldehyde as they dry and cure (Wieslander et al. 1997; Howard et al. 1998; Sherzad and Jung 2022; Hubbe and Laleicke 2025). Such issues can be regarded as having been a primary motivation that explains the present dominance of water-borne coating formulations for products that are applied to wood surfaces in the home or at construction sites of buildings. A study by Dinh et al. (2019) showed rapid release of VOCs during spray application of solvent-based wood coatings; slower release was reported when the same formulations were applied by brush or roll painting. However, in all cases (eight formulations), emissions of VOCs were below the level of detection after 10 hours. These findings agree with those of Fortmann et al. (1998). Lee et al. (2003) evaluated three thicknesses of solvent-based formulation applied to aluminum foil. VOC emissions increased with increasing film thickness, but once again they reached very low levels within 10 hours after application. Wang et al. (2018), in their study of VOC emissions following application of lacquer to veneer particleboard, found that the main contributions to odor fell into the categories of aromatic compounds, aldehydes, and alkanes. Zhu et al. (2016) showed that incorporation of a silane coupling agent and montmorillonite nanoparticles in a waterborne varnish formulation decreased the release of VOCs, especially during the first seven days.

Emissions During Usage of Coated Items

After full curing of coatings for wood, there has been less concern and less study of their related emissions. More study is needed. Analysis of old, flaking paint from buildings suggests that wood coatings may be a major source of release of polychlorinated biphenyls (PCBs) to the air (Jartun et al. 2009).

Some recent trends can contribute to increased concern related to emissions from various materials within homes. As already mentioned, people throughout the world are tending to spend more of their time indoors (Brasche and Bischof 2005). Potential exposure to emissions from wood coatings or other sources has tended to increase due to increased recirculation of indoor air (Nazarenko and Narayanan 2025). Some of the motivation for the increased reuse of indoor air is to reduce costs associated with heating or cooling. The article just cited describes a strategy to overcome such issues by use of heat-exchange technology, thereby increasing air replacement with the outdoors, while minimizing undesired losses or gains in heat.

Types of Volatile Organic Compounds (VOCs)

Oil-based wood coating formulations generally dry by means of evaporation of solvent components, which can be briefly categorized as volatile organic compounds (VOCs). According to Ulker et al. (2021), VOCs are the biggest health concern associated with the usage of indoor furniture. Tests carried out by the cited authors detected styrene, toluene, xylene, ethylbenzene, dichlorobenzene, benzene, and formaldehyde as major components released to the air. Though the wood coating formulations appeared to be the main sources of such emitted compounds, other important contributions were attributed to wood adhesives and natural extractable compounds present in the wood itself. Related work, including additional VOC components and associated health effects, are reviewed by Ulker et al. (2021). The cited authors made a strong endorsement for the usage of powder coatings as a means to minimize VOC issues. As mentioned earlier in this article, the use of UV-curing systems can decrease the reliance upon the evaporation of solvents as a curing mechanism (Gustafsson and Börjesson 2007; Hermann et al. 2021b). Based on a life cycle assessment, Gustafsson and Börjesson (2007) found that a 100% UV lacquer system could be rated as the most environmentally benign option that they considered. A waterborne system came in second in their study.

Though water-borne formulations of wood coatings greatly reduce the usage of organic solvents, they generally do not eliminate them completely (Hubbe and Laleicke 2025). As explained by Flexner (2005), a typical water-borne formulation can be regarded as an emulsion of organic solvent, resins, and pigments in an aqueous phase. As the coating layer dries, after its application, the oil solvent components become sufficiently enriched in the mixture so that they can facilitate the intermixing of polymer segments of adjacent latex particles (Shi et al. 2012; Krongauz 2021; Cabrera et al. 2022). Subsequently, the organic solvents gradually become released as VOCs.

Two-component Systems vs. Emissions

Another approach by which coating formulations have reduced reliance on VOC evaporation is by using pairs of compounds that react with each other. Thus, epoxy resin systems are highly regarded when superior toughness is needed, as for production of wood counter-tops (Salleh et al. 2013). Another example is two-component polyurethane-type systems to which an isocyanate component is mixed prior to application (Chang and Lu 2012, 2013; Ghofrani et al. 2016; Kwon et al. 2024). Obvious drawbacks of such systems include limited usable time after mixing the components, difficulties with cleanup, and generally higher costs than many other coating options. Nevertheless, such reactive or high-solids systems provide opportunities to decrease reliance on volatile carrier liquids. Attention also needs to be paid to possible exposure to unreacted components and to the energy required for curing. Isocyanate compounds, which are used in many polyurethane coatings, also have raised concerns related to health and the environment (Gomez-Lopez et al. 2021). According to a REACH regulation, free isocyanate must be excluded from polyurethane products in the European Union (Gomez-Lopez et al. 2021). As a response, a series of isocyanate-free polyurethane productions have been developed (Zareanshahraki and Mannari 2021).

Sealing by the Coating to Reduce Emissions

Formaldehyde

Engineered wood products, such as fiberboard, particleboard, oriented strand board, and plywood, often contain formaldehyde-based adhesives, and the unintended release of formaldehyde vapor has been an increasing concern. Progress has been reported in preparing such wood products with less formaldehyde emissions (Solt et al. 2019; Antov et al. 2020) or by using formaldehyde-free adhesive options (Hubbe et al. 2018; Goncalves et al. 2021; Kristak et al. 2023). Researchers have considered the possible usage of wood coating as a means to decrease the release of formaldehyde. Table 11 highlights reported findings of such work.

Table 11. Highlights from Studies Concerning Formaldehyde Emissions from Coated Wood, Sometimes Coming from Wood Adhesives

Highlights from Studies Concerning Formaldehyde Emissions from Coated Wood, Sometimes Coming from Wood Adhesives

Sealing for wood preservatives

Wood preservatives, which may include arsenic, pentachlorophenol, and creosote, are also of major concern (Williams et al. 1996). Kukowski et al. (2018) quantified leaching of the highly toxic preservative tebuconazole from both unpainted and painted softwood. Rain-induced leaching was mainly detected as coming from the end grain of the wood. A two-fold reduction in leaching was observed upon application of a water-based primer and one topcoat.

Biobased Sourcing of Wood Coating Components

As a means to decrease usage of petroleum-based substances, there has been some success in using bio-based alternatives. For instance, Wright et al. (2006) showed that polymerized whey proteins could serve as binder resins in wood coatings. Susceptibility to mold growth could be countered by adding biocide. Montazeri and Eckelman (2018) showed favorable results for a 50% bio-renewable content flooring coating formulation that relied on UV curing. Some of the highest projected environmental impacts of the top candidate formulation were associated with the usage of bisphenol A-epichlorohydrin resin and itaconic acid. Etxeberria et al. (2025) formulated new alkyd coatings using bio-based components. High performance was achieved. Such results are consistent with an increasing emphasis on raising the bio-based content of wood coating formulations. It is important, however, to consider possible variations in the renewable feedstocks, together with the durability, biodegradation behavior, and overall life-cycle effects of the resulting coatings.

Lifetime of the Wood Product

Effects of wood finish on product useful lifetime

Extending the useful life of a wood product, assisted either by the durability of an original set of coating layers or as a result of refinishing work, can be counted as an effective way to reduce overall environmental impacts (Jorbandian et al. 2025). Coating durability, and by extension the expected period of usage of an indoor wood item, will depend on a series of choices and efforts that already have been described in this article. In particular, the preservation of appearance and surface quality can be lengthened by attention to optimized sanding, considering the need for a primer coat (depending on the nature of the topcoat selected), and the application of multiple coating layers (Laleicke and Hubbe 2025). Much of the evidence with respect to durability comes from studies of wood exposed to outdoor weather, and there is a need for follow-up studies of coated wood that has been used indoors for different lengths of time.

Figure 17 illustrates the mechanism underlying the popular Taber abrasion test for various solid surfaces (Taber Industries, N.D.). As shown, this device applies a reproducible rubbing action onto selected solid specimens as they are rotated and simultaneously subjected to turning wheels having abrasive surfaces. After running the device for a selected time period, the experimenter inspects the specimen for signs of visible failure and/or weight loss. All efforts related to durability will fail, however, when owners become tired of styles that had been chosen at an earlier stage, often by someone else, in the case of installed wooden cabinets. The good news, from a sustainability perspective, is that organizations such as Habitat Restores often are willing to take the used items and make them available to other customers.

Schematic illustration of key features of the Taber abrasion test device

Fig. 17. Schematic illustration of key features of the Taber abrasion test device

The refinishing of indoor wood items is less common, probably due to the undesirability of sanding dust, organic vapors, and noise happening within a house that is otherwise fully built and may even be presently occupied. Washing of wood with soapy water, followed by wiping dry and then fine-grain sanding of the dry coated wood is recommended as a means to improve adhesion of the new coating to the old one. The washing will remove various monomeric contaminants, such as grease, which otherwise could function as a weak boundary layer between the new and old coating layers (Stehr and Johansson 2000). The sanding will promote mechanical interlocking between the two layers at a microscopic level (Hubbe and Laleicke 2025).

Life-cycle assessment of the coated wood product

Life cycle assessments related to coated wood products have shown a high importance of various end-of-life decisions (Aktas and Bilec 2012). For instance, simple combustion of the material would release carbon dioxide, VOCs, and other contaminants to the atmosphere (Morris 2017; Pelletier et al. 2019). An ideal scenario would use the wood pieces once again in an application similar to the first usage. Though it is possible to consider some intermediate scenarios, such as using the wood material for chipboard or particleboard, such options face challenges related to the presence of coatings on the wood, nails, and various other contaminants.

MECHANISTIC ASPECTS OF FINISHING INDOOR WOOD

This section will focus on three mechanistic aspects that can be important for the coating of indoor wood items. The first topic area is clear coatings, which are a popular way to be able to take advantage of wood’s attractive appearance. The second topic considers the extent to which components of a wood coating may engage in self-assembly phenomena during their application and curing. A third area to be considered is the possibility of specific interactions between components of a coating formulation and the wood components.

Inherent Challenges Associated with Clear Finishes

When a customer of indoor wood products opts for a clear-coated product, that choice immediately imposes a set of inherent challenges. It means, for instance, that the coating must not include any high-refractive-index particles that are large enough to be effective in the scattering of visible light. It follows that if there is a need to protect such wood against the effects of ultraviolet light, then any titanium dioxide particles have to be smaller than about 50 nm or less in diameter, depending on the level of transparency that is needed (Widner and Drummer 2019; Jacucci et al. 2020). According to the cited articles, even if the particles themselves are in the nano range, substantial haze or even opacity can be expected if the particles are present as agglomerates. Care will be required to avoid the creation of bubbles, since their presence will hurt the clarity of the coating. Likewise, any cracks in a clear coating will tend to stand out. Figure 18 shows how the ability of TiO2 and two other kinds of mineral particles to scatter light (considering non-interacting spheres in air) depends on particle diameter (Sigrist Photometer, ND).

Relationship between particle size (spheres in air) vs. diameter for TiO2 (rutile crystal form), alumina, and silica; figure redrawn based on data from Sigrist Photometer

Fig. 18. Relationship between particle size (spheres in air) vs. diameter for TiO2 (rutile crystal form), alumina, and silica; figure redrawn based on data from Sigrist Photometer

In general, cracks are less likely to develop if the formulation contains materials having sufficient extensibility when present in a dried coating (de Meijer and Nienhuis 2009). For example, acrylic latex binders are known for their toughness and resistance to cracking or scratching (Yan et al. 2020c; Tamantini et al. 2023). More inherently brittle coatings can benefit from the inclusion of a plasticizing agent to increase the resistance to cracking over the course of usage (Gutierrezrocca and McGinity 1994).

Refractive index issues

One of the most basic strategies by which to minimize the scattering of light from within a clear coating is to make sure that all components have similar indices of refraction (Kagawa et al. 1998; Zobeiry et al. 2020; Chu et al. 2022). In practice, this requirement is not very hard to achieve. That is because the refractive indices of typical binder resins and minerals such as calcium carbonate tend to fall within a relatively narrow range from about 1.5 to about 1.65. Niskanen et al. (2021) showed that it is feasible to determine the refractive index of particulate materials by examining the light scattering in a varnish medium in the course of a solidification process.

Light scattering by defects and interfacial compatibility issues

Especially when a coating formulation contains mineral fillers, such as calcium carbonate or titanium dioxide, the resulting film can be regarded as a kind of composite. It is well known that the properties of composites are highly dependent on the achievement of efficient wetting and molecular-level adhesion between various phases of material. Especially when there is a strong difference in the Hansen solubility parameters (Hansen 2007) of the respective phases, it is common to observe void areas when inspecting freeze-fractured specimens by electron microscopy (John et al. 2019). Such voids can be evidence of non-contact and non-adhesion at phase boundaries. Another example of strongly incompatible materials, in terms of Hansen solubility principles, involves traditional oil-based varnish and shellac (Waring 1963); the cited author urged users to never apply varnish to a surface that had been primer coated with shellac. Should problems of incompatibility arise during product development of a coating formulation, such difficulties often can overcome such problems by adding a compatibilizing agent, i.e. a compound containing segments that are compatible with each of the respective compatible phases (Lu et al. 2000). Examples include the maleic acid ester of a fatty acid.

Self-assembly Aspects

Orientation of particles

Between the time that a coating formulation is applied to a wood surface and when it has cured, several processes will take place. These processes take place by themselves, on a nanoscale, without the direct involvement of the worker. The processes can include alignment of particles in flow (Jaensson et al. 2016), development of “house-of-cards” structures, interdiffusion of polymer segments between adjacent latex particles, and progressive immobilization of the film. Meanwhile, the one-directional evaporation of the suspending medium during curing of a coating can result in differences of the outer surface from the rest of the coating layer. For instance, amphiphilic compounds or copolymers in the formulation may adopt orientations in which hydrophobic segments become enriched at the air interface. Figure 19 illustrates a variety of factors that are likely to affect self-assembly aspects of especially fibrillar components in not-yet-cured coating formulations.

Illustration of several factors that are likely to affect the self-assembly attributes, including microstructures, of particles within non-yet-cured coating formulations

Fig. 19. Illustration of several factors that are likely to affect the self-assembly attributes, including microstructures, of particles within non-yet-cured coating formulations

Given a sufficient amount of time, in combination with a well-tuned chaotic influence such as eddies of flow or diffusional motions, particles within a formulation can be expected to adopt a thermodynamically preferred structure, which may or may not serve the needs of the formulator. However, dispersed systems frequently adopt non-equilibrium structures along the path to such ideal organizations and then get stuck, for instance due to the curing and solidification of a coating (Hubbe et al. 2023). Figure 20 shows a schematic illustration of particles that are kinetically entrapped in a non-ideal structure that does not represent a minimum in free energy. The question mark in the figure represents a reasonable doubt that real systems will be able to adopt idealized structures, e.g. fully contiguous networks or single perfect crystals, etc. For instance, it is reasonable to expect some rearrangement, at a submicroscopic scale, during the drying and curing of a wood coating.

Representation of kinetically trapped structure resulting from partial or imperfect self-assembly of particles within a suspension, especially in the case of a process in which the suspension becomes immobilized

Fig. 20. Representation of kinetically trapped structure resulting from partial or imperfect self-assembly of particles within a suspension, especially in the case of a process in which the suspension becomes immobilized; figure adapted from a version by the copyright holder (Hubbe et al. 2023)

Zahedi et al. (2018) reviewed the topic of self-stratifying coatings, which can be formulated with different resins such that they would tend to separate into layers upon application. The effects can be achieved by attention to the surface tensions and solubility characteristics of different resins. The process was simulated, using a model that included such factors as surface tensions, viscosities, reaction kinetics, and evaporation rates.

Shear-induced particle alignment and effects of Brownian motion

During the stirring of a coating formulation, and also during the applications of such formulations to wood, hydrodynamic shear forces can be expected to induce transient orientation of any included particles. Such orientation can be predicted by consideration of physical principles (Jeansson et al. 2016). However, due to thermal energy, such alignment usually can be expected to be transient. Depending on the viscosity of the suspending medium, as well as various physical constraints, particles within a non-yet-cured formulation are expected to be undergoing thermally driven random motions that fall under the category of Brownian motion (Hassan et al. 2015). These can include translational motions, which can result in net movement to adjacent places within the mixture. Since diffusion is a slow process, especially for particles larger than molecules, motions in the nanometer range are the main expectation. Particles also undergo rotational Brownian motion (Hassan et al. 2015). As a result of many such motions, there is a likelihood that particles within the mixture will have arranged themselves into a structure that minimizes the net energy of interaction.

Though such a transformation can be thermodynamically favored, it is also very likely that the described self-assembly process becomes stuck as an imperfect immobilized structure that falls short of having achieved a minimization of interaction energy (Hassan et al. 2015). Such systems have been called “kinetically trapped” (Hata et al. 2019; Hubbe et al. 2023; Sellman et al. 2023). Because the viscosity within a freshly applied coating layer will be continually rising, due to the evaporation of the suspending medium and structure forming among various components, such incompletely formed structures can be expected to become essentially frozen into the microstructure of cured coating layers. While these concepts are supported by various evidence (Hubbe et al. 2017), there is a need for more research, especially when it comes to applying them to wood coating practices.

Rheological tests can be carried out as a means to better understand any tendency of transient structures to form and possibly to break up in a coating formulation under controlled conditions of shearing (Hubbe et al. 2017). Such formulations very often exhibit shear-thinning behavior, which can be taken as evidence that either rotational or oscillatory shearing is progressively breaking up various transient structures within the mixture (Hassan et al. 2015). The period of time over which such effects manifest themselves will depend on the rates of the previously mentioned rotational Brownian motions of particles having different sizes and shapes suspended in media that can have differing viscosities.

The very small size of particles and macromolecules within coating formulations can add to the challenge of finding evidence to support various theories related to self-assembly including the effects of flow. Thus, there will be a continuing need for studies using high-resolution and fracture methods to examine the orientations of particles within cured coating layers. Important questions will include not only whether some of the particles retain a favored orientation in the cured coatings, but also whether some such effects have become obscured by subsequent Brownian motion of the particles before immobilization of the coating (Zöttl et al. 2023).

Layer formation

An individual layer of coating that has been freshly applied to a wood surface will experience markedly different conditions at its outer and inner surfaces. The outer surface ordinarily will be exposed to air. The fact that evaporation initially will mainly take place near that surface will create a net flow of the suspending medium in that direction (Hubbe et al. 2023). Binders that are freely suspended in the formulation may be able to follow the flow and thereby become enriched near the outer surface. The near-zero interaction energy provided by a gas phase implies that a low energy state of the surface can be achieved if and when compounds of polymer segments are able to orient themselves such as to enrich the population of low-energy alkyl or aromatic groups facing outwards. A previously applied coating layer of the same type will have undergone a similar process. Therefore, there may be some limited tendency for orientation of the compounds in the freshly applied layer that faces the previous layer, except that such reorientation would be difficult to document or quantify.

Interactions During Application

Most of the important interactions between coating components and wood components are non-covalent in nature. Such interactions will affect the efficiency of wetting, the magnitude of the work of adhesion, and the durability of bonding to the wood. Another kind of interaction can involve the swelling of the wood, especially in the case of waterborne coating formulations. Finally, in this section, some attention will be paid to interactions between coating components and extractable substances present in the wood.

Medium interactions with the wood

Of the three main components of wood, i.e. cellulose, hemicellulose, and lignin, it is the lignin component that has the most similar solubility characteristics to the most commonly used binders that are used in wood coatings (Duval et al. 2016; Zhao et al. 2018;

Ribeiro et al. 2020; Ruwoldt et al. 2022; Ma et al. 2024). As shown by Hansen (2007), the mutual solubility of different pairs of substances can be predicted by comparing their values of their Hildebrand parameter (square-root of the cohesive energy density), their polarity, and their hydrogen bonding ability. These three attributes are illustrated in Fig. 21. Because the outermost electrons are the most polarizable, they are likely to play an over-sized role relative to the Hildebrand parameter. A prime example is the delocalized electrons within aromatic rings and within conjugated (e.g. -C=C-C=C-C=C-) systems. Polar systems arise when a molecule includes atoms having contrasting electronegativities, such as oxygen having a greater electronegativity than carbon. Even though hydrogen bonds involve such differences, Hansen (2007) found that such bonds have such profound effects on solubility behaviors that it is advantageous to consider them separately in solubility calculations.

Representation of the three types of molecular interactions considered in the Hansen solubility theory, namely London dispersion

Fig. 21. Representation of the three types of molecular interactions considered in the Hansen solubility theory, namely London dispersion (related to polarizability of electrons), the polar components of interactions, and the ability to form hydrogen bonds

The best mutual solubility (or surface interactions, if one of the substances is an insoluble solid) is expected when the two substances have similar values of all three of the Hansen solubility parameters. Favorable solubility parameters, in comparison with those of lignin, can help to explain why wood coating often adheres poorly to weathered wood, from which much of the surface lignin has been degraded and washed away (Kropat et al. 2020; Hubbe and Laleicke 2025).

Though it is often stated that cellulose is “polar and hydrophilic” (Miao and Hamad 2019), a more nuanced interpretation has emerged over time. In the wood, cellulose microfibrils are typically surrounded by a sheath of hemicellulose and lignin. In the case of a weathered wood surface, the orientation of the cellulose chains will determine whether the surface is either polar and capable of hydrogen bonding, or non-polar (Yamane et al. 2006). A process of gradual drying in air can be expected to promote transient orientation such that the nonpolar face of cellulose is facing outwards (Hubbe et al. 2023).

Hemicellulose is the most hydrophilic of the main components of wood, but there are reasons to doubt the significance of its possible role in interacting with wood coatings. Modern concepts of wood’s microstructure suggest that much of the hemicellulose constitutes a layer between the cellulose microfibrils in the center and a crust of lignin on the outside. Covalent bonds, which are commonly referred to as lignin-polysaccharide complexes, appear to mainly develop between the lignin and the hemicellulose in the course of biosynthesis of wood. The chemical similarity between cellulose and hemicellulose may mean that covalent bonds are not needed between those two phases to maintain tight cohesion within the wood.

Wetting of wood or of a previous coating layer

The importance of surface cleanliness can be illustrated by considering a wood surface that has been unintentionally contaminated with wax before application of a waterborne coating. In the worst instance, the applied coating might bead up on the excessively hydrophobic surface, leaving much of the wax-coated wood uncovered (Bartolo et al. 2005). Less dramatic versions of the same scenario might be expected in cases where hydrophobic extractable compounds in the wood had migrated to the wood surface over time (Christiansen 1990; Nussbaum 1999; Stehr and Johansson 2000). Such migration is thermodynamically favored due to the relatively low surface energy of such compounds. A thermodynamically favorable situation can be achieved when such compounds are present at air interfaces. The mechanism also explains observed decreases in wettability and poor adhesion to some coatings (Christiansen 1990; Stehr and Johansson 2000). However, some careful measurements have failed to show the expected gradient of chemical position adjacent to the wood surface after thermal treatment (Inari et al. 2006).

Due to the low interfacial tensions of oil media, complete wetting of oil-based formulations on wood surfaces can be expected, even on somewhat greasy surfaces. Though some greasy contaminants on wood, including extractable components of the wood, may serve as a weak boundary layer at the coating interface (Stehr and Johansson 2000), there may be sufficient solubilization and redistribution after application of an oil-based coating in order to minimize problems related to adhesion.

As illustrated in Fig. 22, the wetting of surfaces by water-borne formulations can be improved by judicious addition of surfactants (Swarup and Schoff 1993). Promising surfactants for this purpose are likely to have hydrophile-lipophile balance (HLB) values in the range of about 7 to 9 (Pasquali et al. 2008). Though the cited authors described HLB as an approximate and non-quantitative measure, they admitted that HLB can provide an approximate starting point for formulation work. Further refinement of formulation composition can be achieved by applying the principles of the “hydrophilic-lipophilic deviation model” (Phaodee and Weston 2023), which is based on theories of detergency. In order to accomplish its function as a wetting agent, the additives need to migrate from the bulk of the coating formulation (where it may be partly present as micelles) to the point of wetting.

Illustration of the effect of surfactants within water-borne coating formulations on the wettability of typical wood, especially when the wood is somewhat hydrophobic

Fig. 22. Illustration of the effect of surfactants within water-borne coating formulations on the wettability of typical wood, especially when the wood is somewhat hydrophobic

Diffusion of a surfactant within the aqueous phase of the water-borne coating formulation is likely to be the rate-determining step. Excessive surfactant content in the formulation should be avoided, since it would be expected to detract from the strength of the resulting coating. For instance, excess surfactant present at the interface can be expected to compete with polymer segments of binders for sites of adsorption at a surface (Guillermic and Saint-Jalmes 2013). Though a surfactant in a water-based coating formulation will be a minor ingredient, it can be regarded as an insurance policy, an investment that one makes to guard against possibly skipping the coverage of some areas on the surface.

Figure 23 illustrates the kinds of groups associated with four categories of components of wood, i.e. cellulose, hemicellulose, lignin, and monomeric extractives.

Representation of important functional groups corresponding to the different chemical components of wood

Fig. 23. Representation of important functional groups corresponding to the different chemical components of wood

Although the final category is often much lower in percentage than the three main components, the surface-active nature, and the monomeric form of extractives mean that they are likely to accumulate at surfaces by a process of diffusion. As shown in the figure, the groups associated with both cellulose and hemicellulose are generally polar in nature. Thus, to the extent that the polysaccharide components of wood are dominant at the surface, they favor water-wettability. The groups generally associated with lignin include aromatic rings, which have an intermediate level of wettability by water. Extractives, including rosin acids, fatty acids, and triglyceride fats, are the least water-wettable, such that they may be suspected of playing a key role in cases where wood surfaces are not readily wetted by water-based coatings.

Swelling of the wood

The fact that water causes transient swelling of wood material during the application of waterborne coating can be of heightened concern in indoor applications. As noted in an earlier review (Hubbe and Laleicke 2025), swelling of the wood can cause some of the surface fibers to project outwards. This can give rise to a fuzzy appearance of the coated wood (Flexner 2005). Such problems can be overcome, but time and effort usually are required. For instance, as illustrated in Fig. 24, it has been recommended to pre-wet the surface, allow it to dry, and then gently sand it again with the same fine grain of sandpaper that was the endpoint of the ordinary sanding preparation (Flexner 2005). In theory, application of a water-borne coating formulation to the pre-wetted and sanded wood surface will not exhibit further fiber rise, at least not to the same extent. Bekhta et al. (2002a,b,c) applied such a technique for the finishing of compressed wood. By following this method, one is making the assumption that those fiber segments that were most likely to “rise” would have been removed by the sanding step.

Scheme that can be used to overcome problems of “fiber rise” upon usage of water-borne wood coating, involving pre-wetting, allowing fibers to rise, letting the surface dry, then gentle, fine sanding to remove the raised fibers

Fig. 24. Scheme that can be used to overcome problems of “fiber rise” upon usage of water-borne wood coating, involving pre-wetting, allowing fibers to rise, letting the surface dry, then gentle, fine sanding to remove the raised fibers

Another approach to solving the same problem, as illustrated in Fig. 25, is to start with a water-borne coating formulation, but to interpose a sanding step between the first and second applications. Thus, two coatings, interposed by a sanding step, will be required to achieve a surface within which there are no fiber ends. An advantage of such an approach is that the first layer of coating, after it has cured, will greatly reduce further interactions of the applied water in the next coating application with the underlying wood.

Primer coatings can be formulated such as to reduce the tendency for swelling of surface fibers (sometimes called “grain puffing”) upon applications of subsequent waterborne coating layers (Duan and Fan 2021; Yang and Ke 2022). For instance, this was achieved by inclusion of a siloxane component with a hydrophobic group.

Strategy to deal with fiber rise by allowing it to happen upon addition of a first layer of water-borne coating, applying gentle sanding after drying of the coating, and then applying a second coat (not shown)

Fig. 25. Strategy to deal with fiber rise by allowing it to happen upon addition of a first layer of water-borne coating, applying gentle sanding after drying of the coating, and then applying a second coat (not shown)

Though practitioners are often aware of negative consequences of the swelling of wood by water, there is also an expected benefit. Surface swelling of the wood, upon application of a water-borne formulation, will increase access of binder macromolecules into spaces between fibers. This will result in an increased area of interaction on a microscopic scale, making the later peeling of the first coating layer to be applied less likely. Research is needed to clarify such a mechanism and to determine its relative importance.

Interactions with extractives

Some of the clearest evidence of the impact of wood extractives on varnish coating of wood was obtained by optimally extracting alder and ironwood surfaces using hot water and ethanol (Ghofrani et al. 2016). Extracted wood surfaces showed higher adhesion strength. The effects were partly attributed to increased water-wettability of the wood surfaces, due to higher free energy of the surface.

CONCLUSIONS

  1. Based on publications cited in this review, it can be concluded that a great deal is already known about the coating of wood for indoor applications. Much of this information comes from experts who have devoted a long time not only to theories but also to practical experiences with the application and effects of such treatments of wood. The basic knowledge continues to be richly supplemented by fresh research findings.
  2. Though there are some ways in which the coating of wood contributes to adverse environmental impacts, there is an overall reduction in life cycle concerns due to the fact that wood coating can promote the durability and increased usage of wood, including its usage in the interiors of buildings.
  3. There are many opportunities for research in the general area of interior wood coatings. The research field has suffered some limitations for many years during which there has been an emphasis on new materials, such as plastics, for interior usage. In addition, many researchers have opted to study exterior wood coating applications, which present special challenges. The immediate future appears to be favorable for a renewed focus on interior wood coating, due to concerns such as air quality, aesthetics of interior spaces, and the minimization of overall environmental impacts by the usage of wood. Priority research questions include standardized indoor-aging protocols; long-term VOC, SVOC, particulate, and microplastic release; coating–wood interactions across species; durability and life-cycle performance of bio-based systems; and scalable sensing, automation, and digital control. Increasing use of exposed structural timber and engineered wood products also creates needs related to moisture cycling, intermittent condensation, maintenance and recoating, compatibility with fire-protection requirements, and retention of appearance during long indoor service. Field validation is needed to connect accelerated tests with actual service life.

ACKNOWLEDGEMENTS

The authors acknowledge support from an endowment grant from the Buckman Foundation. The authors also are grateful for the help from the following experts who participated in an open peer-review process, involving an earlier version of this article: Redzuan Mohammad Suffian James, Institute of Tropical Forestry and Forest Products (INTROP), Universiti Putra Malaysia, 43400 UPM Serdang, Selangor, Malaysia; Ahmet Cihangir Yalinkilic, Department of Industrial Design Engineering, Simav Technology Faculty, Kutahya Dumlupinar University, Kutahya, Türkiye; Seungmin Yang, Chungnam National University, 34134, 99 Daehak-ro,Yuseong-gu, Daejeon, Republic of Korea; Milan Sernek, Biotechnical Faculty, University of Ljubljana, Jamnikarjeva 101, Ljubljana 1000, Slovenia; Mehmet Budakçı, Department of Wood Products Industrial Engineering, Faculty of Forestry, Düzce University; 81060, Düzce, Türkiye; and Xianping Wang, Senior Principal Scientist and R&D Manager for Engineered Wood Products, Bostic.

REFERENCES CITED

Abdulkareem, S., Orkuma, G. I., and Apasi, A. A. (2010). “Talc as a substitute for dry lubricant (an overview),” in: International Conference on Advances in Materials and Processing Technologies, F. Chinesta, et al. (eds.), AIP Conf. Proceedings, Vol. 1315, pp. 1400-1404. https://doi.org/10.1063/1.3552382

Acarali, N., and Demir, S. (2021). “Physical and chemical effects of quartet structure (bamboo/zinc borate/shellac/surfactant) on organic coatings,” J. Indian Chem. Soc. 98(3), article 100043. https://doi.org/10.1016/j.jics.2021.100043

Aguilar, C. N., Rodriguez, R., Gutierrez-Sanchez, G., Augur, C., Favela-Torres, E., Prado-Barragan, L. A., Ramirez-Coronel, A., and Contreras-Esquivel, J. C. (2007). “Microbial tannases: Advances and perspectives,” Appl. Microbiol. Biotechnol. 76, 47-59. https://doi.org/10.1007/s00253-007-1000-2

Akbari, V., Vanslambrouck, S., and Landry, V. (2025). “Enhancing wood hardness through surface impregnation via Michael addition: A study on penetration patterns of three North American hardwoods,” Eur. J. Wood Wood Prod. 83(3), article 122. https://doi.org/10.1007/s00107-025-02263-7

Akiyama, R., Mori, T., Aoyama, H., and Oya, T. (2014). “Study on method to generate wood grain pattern representing required impression,” in: Proceedings of the ASME International Design Engineering Technical Conferences and Computers and Information in Engineering Conference, 2013, Vol. 2A, ASME, article V02AT02A051. https://doi.org/10.1115/DETC2013-12508

Aksu, S., Kelleci, O., Aydemir, D., and Istek, A. (2022). “Application of acrylic-based varnishes reinforced with nano fillers for conservation of weathered and worn surfaces of the historical and cultural wooden buildings,” J. Cultural Heritage 54, 1-11. https://doi.org/10.1016/j.culher.2022.01.003

Aktas, C. B., and Bilec, M. M. (2012). “Service life prediction of residential interior finishes for life cycle assessment,” Int. J. Life Cycle Assess. 17(3), 362-371. https://doi.org/10.1007/s11367-011-0367-6

Allen, S. (1984). Wood Finisher’s Handbook, Sterling Pub. Co., New York.

Ansari, F., Ries, M. D., and Pruitt, L. (2016). “Effect of processing, sterilization and crosslinking on UHMWPE fatigue fracture and fatigue wear mechanisms in joint arthroplasty,” J. Mechan. Behav. Biomed. Mater. 53, 329-340. https://doi.org/10.1016/j.jmbbm.2015.08.026

Antov, P., Savov, V., and Neykov, N. (2020). “Reduction of formaldehyde emission from engineered wood panels by formaldehyde scavengers – A review,” in: Sustainability of Forest-Based Industries in the Global Economy, D. Jelacic (ed.), pp. 289-294.

Aprianti, N., Kismanto, A., Supriatna, N. K., Yarsono, S., Nainggolan, L. M. T., Purawiardi, R. I., Fariza, O., Ermada, F. J., Zuldian, P., and Raksodewanto, A. A. (2023). “Prospect and challenges of producing carbon black from oil palm biomass: A review,” Bioresour. Technol. Rep. 23, article 101587. https://doi.org/10.1016/j.biteb.2023.101587

Areias, L. R. P., and Farinha, J. P. S. (2023). “Waterborne polymer coatings with bright noniridescent structural colors,” ACS Appl. Mater. Interfaces 16(1), 1587-1595. https://doi.org/10.1021/acsami.3c16290

Arrais, R., Costa, C. M., Ribeiro, P., Rocha, L. F., Silva, M., and Veiga, G. (2021). “On the development of a collaborative robotic system for industrial coating cells,” International Journal of Advanced Manufacturing Technology 115, 853-871. https://doi.org/10.1007/s00170-020-06167-z

Atilgan, A., and Sofuoglu, S. D. (2023). “The effect of hot and cold check tests on surface roughness and glossiness in varnished wood material,” Drvna Industrija 74(4), 395-406. https://doi.org/10.5552/drvind.2023.0085

Auclair, N., Riedl, B., Blanchard, V., and Blanchet, P. (2011). “Improvement of photoprotection of wood coatings by using inorganic nanoparticles as ultraviolet absorbers,” Forest Prod. J. 61(1), 20-27. https://doi.org/10.13073/0015-7473-61 1.20

Ayata, Ü., and Çakicier, N. (2021). “Determination of pendulum hardness (Konig method) values against artificial weathering in water-based varnishes applied to some wood species after heat treatment (thermowood),” Drewno 64(208). https://doi.org/10.12841/wood.1644-3985.381.06

Bai, J., Li, Y., Jiang, S. S., and Guan, H. Y. (2022). “Preparation of wood furniture cooling coatings based on phase change microcapsules and its performance study,” BioResources 17(1), 1319-1337. https://doi.org/10.15376/biores.17.1.1319-1337

Bansal, R., Nair, S., and Pandey, K. K. (2022). “UV resistant wood coating based on zinc oxide and cerium oxide dispersed linseed oil nano-emulsion,” Mater. Today Commun. 30, article 103177. https://doi.org/10.1016/j.mtcomm.2022.103177

Bartolo, D., Josserand, C., and Bonn, D. (2005). “Retraction dynamics of aqueous drops upon impact on non-wetting surfaces,” J. Fluid Mechan. 545, 329-338. https://doi.org/10.1017/S0022112005007184

Bauer, F., Decker, U., Czihal, K., Mehnert, R., Riedel, C., Riemschneider, M., Schubert, R., and Buchmeiser, M. R. (2009). “UV curing and matting of acrylate nanocomposite coatings by 172 nm excimer irradiation,” Progress in Organic Coatings 64(4), 474-481. https://doi.org/10.1016/j.porgcoat.2008.08.009

Bazin, C., Beurdeley, P., Lefevre, F., Camara, F., and Roidot, C. (2026). “Polymer dispersion for coating wood for blocking migratable compounds,” US Patent 12577329 B2.

Bekhta, P., Krystofiak, T., Lis, B., and Bekhta, N. (2022a). “The impact of sanding and thermal compression of wood, varnish type and artificial aging in indoor conditions on the varnished surface color,” Forests 13(2), article 300. https://doi.org/10.3390/f13020300

Bekhta, P., Lis, B., Krystofiak, T., and Bekhta, N. (2022b). “Surface roughness of varnished wood pre-treated using sanding and thermal compression,” Forests 13(5), article 777. https://doi.org/10.3390/f13050777

Bekhta, P., Lis, B., Krystofiak, T., Tokarczyk, M., and Bekhta, N. (2022c). “Gloss of varnished MDF panels veneered with sanded and thermally compressed veneer,” Coatings 12(7), article 913. https://doi.org/10.3390/coatings12070913

Bible, R. C., and Johnson, N. (2002). “Retroreflective material specifications and on-road sign performance,” in: Traffic Control Devices, Visibility, and Rail-Highway Grade Crossings 2002, Book Ser. Transportation Research Record, Issue 1801, pp. 61-72. https://doi.org/10.3141/1801-08

Boehme, C. (1995). “Reducing formaldehyde emission of UF-bonded particleboards using blocking layers,” Holz Roh- Werkstoff 53(4), 237-242. https://doi.org/10.1007/s001070050079

Boivin, G., Ritcey, A. M., and Landry, V. (2019). “The effect of silver nanoparticles on the black-stain resistance of acrylic resin for translucent wood coating application,” BioResources 14(3), 6353-6369. https://doi.org/10.15376/biores.14.3.6353-6369

Brasche, S., and Bischof, W. (2005). “Daily time spent indoors in German homes – Baseline data for the assessment of indoor exposure of German occupants,” Int. J. Hygiene Environ. Health 208(4), 247-253. https://doi.org/10.1016/j.ijheh.2005.03.003

Broda, M., Jakes, J. E., Li, L. X., and Antipova, O. A. (2023). “Archeological wood conservation with selected organosilicon compounds studied by XFM and nanoindentation,” Wood Sci. Technol. 57(6), 1277-1298. https://doi.org/10.1007/s00226-023- 01503-4

Budakçı, M., Sönmez, A. and Pelit, H. (2012). “The color changing effect of the moisture content of wood materials on water borne varnishes,” BioResources 7(4), 5448-5459. https://doi.org/10.15376/biores.7.4.5448-5459

Buxbaum, G., and Pfaff, G. (2005). Industrial Inorganic Pigments, 3rd Ed., Wiley-WCH, Weinheim, Germany. https://doi.org/10.1002/3527603735

Cabrera, I., Rückel, M., Boyko, V., Baumstark, R., and Willerich, I. (2022). “Quick curing mechanisms for all-season paints and renders,” Materials 15(20), article 7397. https://doi.org/10.3390/ma15207397

Çakicier, N., Korkut, S., and Korkut, D. S. (2011). “Varnish layer hardness, scratch resistance, and glossiness of various wood species as affected by heat treatment,” BioResources 6(2), 1648-1658. https://doi.org/10.15376/biores.6.2.1648-1658

Cefla Finishing (2022). “Excimer technology: Innovative UV finishing for matt surfaces.” https://www.ceflafinishing.com/en/magazine/excimer-technology-flat-raised-panel-matting

Chadwick, A. C., and Kentridge, R. W. (2015). “The perception of gloss: A review,” Vision Res. 109, 221-235. https://doi.org/10.1016/j.visres.2014.10.026

Chang, C. W., and Lu, K. T. (2012). “Natural castor oil based 2-package waterborne polyurethane wood coatings,” Prog. Organic Coat. 75(4), 435-443. https://doi.org/10.1016/j.porgcoat.2012.06.013

Chang, C. W., and Lu, K. T. (2013). “Linseed-oil-based waterborne UV/air dual-cured wood coatings,” Prog. Organic Coat. 76(7-8), 1024-1031. https://doi.org/10.1016/j.porgcoat.2013.02.020

Chen, H., Montanari, C., Shanker, R., Marcinkevicius, S., Berglund, L. A., and Sychugov, I. (2022). “Photon walk in transparent wood: Scattering and absorption in hierarchically structured materials,” Advan. Optical Mater. 10(8), article 2102732. https://doi.org/10.1002/adom.202102732

Christiansen, A. W. (1990). “How overdrying wood reduces its bonding to phenol-formaldehyde adhesives – A critical-review of the literature. 1. Physical responses,” Wood Fiber Sci. 22(4), 441-459.

Chu, T. Y., Gao, Y. X., Yi, L., Fan, C. G., Yan, L., Ding, C., Liu, C. C., Huang, Q., and Wang, Z. Y. (2022). “Highly fire-retardant optical wood enabled by transparent fireproof coatings,” Advan. Composites Hybrid Mater. 5(3), 1821-1829. https://doi.org/10.1007/s42114-022-00440-3

CIE. (2018). Colorimetry, 4th Ed., CIE 015:2018, International Commission on Illumination, Vienna, Austria. https://doi.org/10.25039/TR.015.2018

Colombini, M. P., Andreotti, A., Baraldi, C., Degano, I., and Lucejko, J. J. (2007). “Colour fading in textiles: A model study on the decomposition of natural dyes,” Microchem. J. 85(1), 174-182. https://doi.org/10.1016/j.microc.2006.04.002

Cong, H. L., Yu, B., Wang, S. P., Qi, L. M., Wang, J. L., and Ma, Y. R. (2013). “Preparation of iridescent colloidal crystal coatings with variable structural colors,” Optics Express 21(15), 17831-17838. https://doi.org/10.1364/OE.21.017831

Cox, R. M. (2003). Building an Industrial Wood Finish, Forest Products Society, Madison, WI.

Cuppo, F. L. S., García-Valenzuela, A., and Olivares, J. A. (2013). “Influence of surface roughness on the diffuse to near-normal viewing reflectance factor of coatings and its consequences on color measurements,” Color Res. Appl. 38(3), 177-187. https://doi.org/10.1002/col.20752

Czachor-Jadacka, D., Pilch-Pitera, B., Kisiel, M., and Gumieniak, J. (2021). “Hydrophobic UV-curable powder clear coatings: Study on the synthesis of new crosslinking agents based on raw materials derived from renewable sources,” Mater. 14(16), article 4710. https://doi.org/10.3390/ma14164710

Deline, V. R., Brown, H. R., and Char, K. (1991). “The use of secondary ion mass-spectrometry to investigate copolymer enhanced adhesion between immiscible polymers,” J. Vacuum Sci. Technol. A – Vac. Surf. Films 9(3), 1283-1286. https://doi.org/10.1116/1.577613

de Meijer, M., and Nienhuis, J. (2009). “Influence of internal stress and extensibility on the exterior durability of wood coatings,” Prog. Organic Coatings 65(4), 498-503. https://doi.org/10.1016/j.porgcoat.2009.04.011

Dietz, P. F. (2023). “Examining the efficiency of titanium dioxide in matt paints and methods of obtaining optimal dry opacity without sacrificing wet hide,” Surf. Coat. Int. 106(5), 342-348.

Ding, W. B., Li, W. Y., Gao, Q., Han, C. R., Zhang, S. F., and Li, J. Z. (2013). “The effects of sealing treatment and wood species on formaldehyde emission of plywood,” BioResources 8(2), 2568-2582. https://doi.org/10.15376/biores.8.2.2568-2582

Dinh, T. V., Son, Y. S., Choi, I. Y., Song, K. Y., Sunwoo, Y., and Kim, J. C. (2019). “Emissions of volatile organic compounds associated with painting methods and an estimation of the α-dicarbonyl formation potential,” Int. J. Environ. Sci. Technol. 16(8), 3961-3970. https://doi.org/10.1007/s13762-018-2100-5

Dizman, C., and Ozman, E. (2020). “Preparation of rapid (chain-stopped) alkyds by incorporation of gum rosin and investigation of coating properties,” Turkish J. Chem. 44(4), 932-940. https://doi.org/10.3906/kim-2001-56

Drelich, J., and Miller, J. D. (1995). “A critical review of wetting and adhesion phenomena in the preparation of polymer-mineral composites,” Minerals Metallurg. Processing 12(4), 197-204. https://doi.org/10.1007/BF03403103

Drupitha, M. M., Misra, M., and Mohanty, A. K. (2023). “Recent advances on value-added biocarbon preparation by the pyrolysis of renewable and waste biomass, their structure and properties: A move toward an ecofriendly alternative to carbon black,” Environ. Sci. Advan. 2(10), 1282-1301. https://doi.org/10.1039/d3va00107e

Duan, G., and Fan, S.-G. (2021). “Use of aqueous dispersion of siloxane for reducing grain puffing of wood substrate and article comprising anti-grain puffing coating,” US Patent 11198230 B2.

Duval, A., Vilaplana, F., Crestini, C., and Lawoko, M. (2016). “Solvent screening for the fractionation of industrial kraft lignin,” Holzforschung 70(1), 11-20. https://doi.org/10.1515/hf-2014-0346

Dvorák, O., Pánek, M., Kvietková, M. S., Pastierovic, F., Sterbová, I., Kubista, K., and Sahula, L. (2023). “Influence of wood species on quality of exterior transparent acrylic coating during outdoor exposure,” Wood Res. 67(6), 994-1004. https://doi.org/10.37763/wr.1336-4561/67.6.9941004

Eley, R. R. (2019). “Applied rheology and architectural coating performance,” Journal of Coatings Technology and Research 16, 263-305. https://doi.org/10.1007/s11998-019-00187-5.

Elliott, P. T., Steffenhagen, M. J., and Glass, J. E. (2007). “Spray applications: Part III. Assessment of viscosities at high shear rates and dynamic uniaxial extensional viscosities on fan nozzle air sprayability,” Journal of Coatings Technology and Research 4, 341-349. https://doi.org/10.1007/s11998-007-9050-z

ElKabbash, M., Hoffman, N., Lininger, A. R., Jalil, S. A., Letsou, T., Hinczewski, M., Strangi, G., and Guo, C. L. (2023). “Fano resonant optical coatings platform for full gamut and high purity structural colors,” Nature Commun. 14(1), article 3960. https://doi.org/10.1038/s41467-023-39602-2

El Messiry, M., and Fadel, N. (2020). “Enhancing the spreading dynamics of oil drops over nanofiber substrates,” Textile Res. J. 90(2), 213-226. https://doi.org/10.1177/0040517519866947

Ersoy, O., Fidan, S., Köse, H., Guler, D., and Özdöver, Ö. (2021). “Effect of calcium carbonate particle size on the scratch resistance of rapid alkyd-based wood coatings,” Coatings 11(3), article 340. https://doi.org/10.3390/coatings11030340

Evans, P. D., Haase, J. G., Shakri, B. M. S. A., and Kiguchi, M. (2015). “The search for durable exterior clear coatings for wood,” Coatings 5(4), 830-864. https://doi.org/10.3390/coatings5040830

Etxeberria, I., Svensson, I., Díaz, A. I., and Barruetabeña, L. (2025). “Novel bio-based formulations for alkyd wood coatings: Effects on biodegradation and technical performance,” Coatings 15(4), article 400. https://doi.org/10.3390/coatings15040400

Faiyad, A., Miliate, D., Leventini, S., Lince, J. R., and Martini, A. (2025). “Temperature-dependent friction, wear, and life of MoS2 dry film lubricants for space mechanisms: A comprehensive review,” Tribology Lett. 73(4), article 114. https://doi.org/10.1007/s11249-025-02052-6

Flexner, B. (1994). Understanding Wood Finishing: How to Select and Apply the Right Finish, Rodale Press, New York.

Flexner, B. (2005). Understanding Wood Finishing: How to Select and Apply the Right Finish, Readers Digest, Pleasantville, NY.

Forsthuber, B., Schaller, C., and Grüll, G. (2013). “Evaluation of the photo stabilising efficiency of clear coatings comprising organic UV absorbers and mineral UV screeners on wood surfaces,” Wood Sci. Technol. 47(2), 281-297. https://doi.org/10.1007/s00226-012-0487-6

Fortmann, R., Roache, N., Chang, J. C. S., and Guo, Z. (1998). “Characterization of emissions of volatile organic compounds from interior alkyd paint,” J. Air Waste Manag. Assoc. 48(10), 931-940. https://doi.org/10.1080/10473289.1998.10463741

Gaff, M., and Gasparík, M. (2013). “The development of stresses during the shaping of the surface of aspen wood and their impact on the quality of the surface,” BioResources 8(3), 3741-3752. https://doi.org/10.15376/biores.8.3.3741-3752

Gaff, M., Gasparík, M., and Kvietková, M. (2017). “Evaluation of wood surface quality depending on the embossing parameters,” Wood Res. 62(5), 751-762. https://doi.org/10.15376/biores.8.3.3741-3752

Gertzmann, R., Nazaran, P., Garcia Martinez, J. M., and Almato Guiteras, M. (2017). “Aqueous acrylic coating system and method for improving the appearance of grained wood surfaces,” US Patent 9624387 B2.

Ghofrani, M., Mirkhandouzi, F. Z., and Ashori, A. (2016). “Effects of extractives removal on the performance of clear varnish coatings on boards,” J. Composite Mater. 50(21), 3019-3024. https://doi.org/10.1177/0021998315615205

Goktas, O., Bozkaya, Y. T., and Yeniocak, M. (2023a). “The use of herbal extracts in lacquer paint coloring and determination of some mechanical resistance properties on wood-based surfaces,” Maderas – Cienncia y Tecnologia 25, article 31. https://doi.org/10.4067/s0718-221×2023000100431

Goktas, O., Bozkaya, Y. T., and Yeniocak, M. (2023b). “Coloration of lacquered coatings for furniture production with herbal dyes and determining weathering resistance,” Drvna Industrija 74(2), 205-212. https://doi.org/10.5552/drvind.2023.0050

Gomez-Lopez, A., Panchireddy, S., Grignard, B., Calvo, I., Jerome, C., Detrembleur, C., and Sardon, H. (2021). “Poly(hydroxyurethane) adhesives and coatings: State-of-the-art and future directions,” ACS Sustain. Chem. Eng. 9(29), 9541-9562. https://doi.org/10.1021/acssuschemeng.1c02558

Goncalves, D., Bordado, J. M., Marques, A. C., and dos Santos, R. G. (2021). “Non-formaldehyde, bio-based adhesives for use in wood-based panel manufacturing industry – A review,” Polymers 13(23), article 4086. https://doi.org/10.3390/polym13234086

Gratzl, J. S. (1985). “Lichtinduzierte Vergilbung von Zellstoffen – Ursachen und Verhütung,” Das Papier 39(10A), 14-23.

Grüll, G., Tscherne, F., Spitaler, I., and Forsthuber, B. (2014). “Comparison of wood coating durability in natural weathering and artificial weathering using fluorescent UV-lamps and water,” Eur. J. Wood Wood Prods. 72(3), 367-376. https://doi.org/10.1007/s00107-014-0791-y

Guasti, M. F., and Diamant, R. (2012). “Generalized Snell’s refraction angle relationship,” Optica Pura y Aplicada 45(3), 377-385. https://doi.org/10.7149/OPA.45.3.377

Guillermic, R. M., and Saint-Jalmes, A. (2013). “Dynamics of poly-NIPAM chains in competition with surfactants at liquid interfaces: From thermoresponsive interfacial rheology to foams,” Soft Matter 9(4), 1344-1353. https://doi.org/10.1039/c2sm26666k

Gupta, B. S., Jelle, B. P., Hovde, P. J., and Gao, T. (2015). “Wood coating failures against natural and accelerated climates,” Proc. Inst. Civil Eng. – Construct. Mater. 168(1), article 1300022. https://doi.org/10.1680/coma.13.00022

Gustafsson, L. M., and Börjesson, P. (2007). “Life cycle assessment in green chemistry: A comparison of various industrial wood surface coatings,” Int. J. Life Cycle Assess. 12(3), 151-159. https://doi.org/10.1065/lca2006.11.280

Gutierrezrocca, J. C., and McGinity, J. W. (1994). “Influence of water-soluble and insoluble plasticizers on the physical and mechanical properties of acrylic resin copolymers,” Int. J. Pharma 103(3), 293-301. https://doi.org/10.1016/0378-5173(94)90180-5

Halstensen, M., Agu, O. V., Hundhausen, U., and Esbensen, K. H. (2021). “Real-time monitoring of wood cladding spray painting properties and nozzle condition using acoustic chemometrics,” Linköping Electronic Conference Proceedings 176, 352-359. https://doi.org/10.3384/ecp20176352

Hansen, C. M. (2007). Hansen Solubility Parameters: A User’s Handbook, 2nd Ed., CRC Press, Boca Raton, FL. https://doi.org/10.1201/9781420006834

Hassan, P. A., Rana, S., and Verma, G. (2015). “Making sense of Brownian motion: Colloid characterization by dynamic light scattering,” Langmuir 31(1), 3-12. https://doi.org/10.1021/la501789z

Hata, Y., Sawada, T., Marubayashi, H., Nojima, S., and Serizawa, T. (2019). “Temperature-directed assembly of crystalline cellulose oligomers into kinetically trapped structures during biocatalytic synthesis,” Langmuir 35(21), 7026-7034. https://doi.org/10.1021/acs.langmuir.9b00850

Hauptmann, M., Müller, U., Obersriebnig, M., Gindl-Altmutter, W., Beck, A., and Hansmann, C. (2013). “The optical appearance of wood related to nanoscale surface roughness,” BioResources 8(3), 4038-4045. https://doi.org/10.15376/biores.8.3.4038-4045

He, Y. Y., Liu, L. Y., Fu, Q. Q., and Ge, J. P. (2022). “Precise assembly of highly crystalline colloidal photonic crystals inside the polyester yarns: A spray coating synthesis for breathable and durable fabrics with saturated structural colors,” Advan. Func. Mater. 32(24), article 2200330. https://doi.org/10.1002/adfm.202200330

He, Z.-B., Ni, Y.-H., and Zhang, E. (2004). “Alkaline darkening and its relation to peroxide bleahcing of mechanical pulp,” J. Wood Chem. Technol. 24(1), 1-12. https://doi.org/10.1081/WCT-120035940

Hendy, S. (2002). “Light scattering in transparent glass ceramics,” Appl. Phys. Lett. 81(7), 1171-1173. https://doi.org/10.1063/1.1499989

Hermann, A., Burr, D., and Landry, V. (2020). “Comparative study of the impact of additives against oxygen inhibition on pendulum hardness and abrasion resistance for UV-curable wood finishes,” Prog. Organ. Coatings 148, article 105879. https://doi.org/10.1016/j.porgcoat.2020.105879 (first published version)

Hermann, A., Burr, D., and Landry, V. (2021a). “Comparative study of the impact of additives against oxygen inhibition on pendulum hardness and abrasion resistance for UV-curable wood finishes,” Prog. Organ. Coatings 156, article 106266. https://doi.org/10.1016/j.porgcoat.2021.106266 (second published version with minor updates)

Hermann, A., Giljean, S., Pac, M. J., Marsiquet, C., Beaufils-Marquet, M., Burr, D., and Landry, V. (2021b). “Understanding indentation, scratch and wear behavior of UV-cured wood finishing products,” Prog. Oran. Coatings 161, article 106504. https://doi.org/10.1016/j.porgcoat.2021.106504

Howard, E. M., McCrillis, R. C., Krebs, K. A., Fortman, R., Lao, H. C., and Guo, Z. (1998). “Indoor emissions from conversion varnishes,” J. Air Waste Manag. Assoc. 48(10), 924-930. https://doi.org/10.1080/10473289.1998.10463747

Huang, J. D., Li, M. M., Ren, C. Y., Huang, W. T., Miao, Y., Wu, Q., and Wang, S. Q. (2022). “Construction of HLNPs/Fe3O4 based superhydrophobic coating with excellent abrasion resistance, UV resistance, flame retardation and oil absorbency,” J. Environ. Chem. Eng. 11(1), article 109046. https://doi.org/10.1016/j.jece.2022.109046

Hubbe, M. A., Gardner, D. J., and Shen, W. (2015). “Contact angles and wettability of cellulosic surfaces: A review of proposed mechanisms and test strategies,” BioResources 10(4), 8657-8749. https://doi.org/10.15376/biores.10.4.8657-8749

Hubbe, M. A., and Laleicke, F. (2025). “Chemical and mechanistic aspects of wood finishing: A review encompassing paints and clear coats,” BioResources 20(2), 4962-5029. https://doi.org/10.15376/biores.20.2.Hubbe

Hubbe, M. A., Pizzi, A., Zhang, H. Y., and Halis, R. (2018). “Critical links governing performance of self-binding and natural binders for hot-pressed reconstituted lignocellulosic board without added formaldehyde: A review,” BioResources 13(1), 2049-2115. https://doi.org/10.15376/biores.13.1.Hubbe

Hubbe, M. A., Rojas, O. J., Fingas, M., and Gupta, B. S. (2013). “Cellulosic substrates for removal of pollutants from aqueous systems: A review. 3. Spilled oil and emulsified organic liquids,” BioResources 8(2), 3038-3097. https://doi.org/10.15376/biores.8.2.3038-3097

Hubbe, M. A., Tayeb, P., Joyce, M., Tyagi, P., Kehoe, M., Dimic-Misic, K., and Pal, L. (2017). “Rheology of nanocellulose-rich aqueous suspensions: A review,” BioResources 12(4), 9556-9661. https://doi.org/10.15376/biores.12.1.2143-2233

Hubbe, M. A., Trovagunta, R., Zambrano, F., Tiller, P., and Jardim, J. (2023). “Self-assembly fundamentals in the reconstruction of lignocellulosic materials: A review,” BioResources 18(2), 4262-4331. https://doi.org/10.15376/biores.18.2.Hubbe

Hundhausen, U., Mai, C., Slabohm, M., Gschweidl, F., and Schwarzenbrunner, R. (2020). “The staining effect of iron (II) sulfate on nine different wooden substrates,” Forests 11(6), article 658. https://doi.org/10.3390/f11060658

Husić, I., Mahendran, A. R., Sinic, J., Jocham, C., and Lammer, H. (2023). “Interaction of porous substrate and vegetable oil-based hydrophobic thermoset coatings during UV-polymerization,” J. Plastic Film Sheeting 39(4), 427-446. https://doi.org/10.1177/87560879231190574

Hysek, S., Fidan, H., Pánek, M., Böhm, M., and Trgala, K. (2018). “Water permeability of exterior wood coatings: Waterborne acrylate dispersions for windows,” J. Green Building 13(3), 3-16. https://doi.org/10.3992/1943-4618.13.3.1

Inari, G. N., Petrissans, M., Lambert, J., Ehrhardt, J. J., and Gérardin, P. (2006). “XPS characterization of wood chemical composition after heat-treatment,” Surf. Interface Anal. 38(10), 1336-1342. https://doi.org/10.1002/sia.2455

Ivanov, L. A., Kiselev, N. N., Slugin, V. A., Kiesewetter, D. V., and Malyugin, V. I. (2006). “Measuring the retroreflection from glass microspheres and predicting the quality of retroreflective coatings,” J. Optical Technol. 73(1), 29-33. https://doi.org/10.1364/JOT.73.000029

Jacucci, G., Schertel, L., Zhang, Y. T., Yang, H., and Vignolini, S. (2020). “Light management with natural materials: From whiteness to transparency,” Advan. Mater. 33(28), article 2001215. https://doi.org/10.1002/adma.202001215

Jaensson, N. O., Hulsen, M. A., and Anderson, P. D. (2016). “Direct numerical simulation of particle alignment in viscoelastic fluids,” J. Non-Newtonian Fluid Mechan. 235, 125-142. https://doi.org/10.1016/j.jnnfm.2016.07.008

James, J. M., and Taifa, I. W. R. (2023). “Quality improvement of long oil alkyd (LOA) resin requirements in the formulation of Hi-gloss paints,” Int. J. Qual. Reliab. Manag. 40(7), 1753-1776. https://doi.org/10.1108/IJQRM-08-2022-0247

Jartun, M., Ottesen, R. T., Steinnes, E., and Volden, T. (2009). “Painted surfaces – Important sources of polychlorinated biphenyls (PCBs) contamination to the urban and marine environment,” Environ. Pollut. 157(1), 295-302. https://doi.org/10.1016/j.envpol.2008.06.036

John, R., Schreiter, K., Trommler, K., Siegel, C., Wagenführ, A., and Spange, S. (2019). “Maleic anhydride copolymers as adhesion-promoting reagent in wood veneer/ biopolyethlyene composite materials,” Polym. Composites 40(5), 1979-1988. https://doi.org/10.1002/pc.24974

Jorbandian, A., Ashori, A., and Jonoobi, M. (2025). “High-performance and sustainable clear water-based coatings for outdoor wood protection: A review,” Prog. Organic Coatings 208, article 109452. https://doi.org/10.1016/j.porgcoat.2025.109452

Kagawa, Y., Iba, H., Tanaka, M., Sato, H., and Chang, T. (1998). “Fabrication and optical/thermal properties of glass particle-epoxy optically transparent composites,” Acta Mater. 46(1), 265-271. https://doi.org/10.1016/S1359-6454(97)00190-0

Kardar, P., and Amini, R. (2022). “Influence of surface preparations of wood on the wetting and adhesion of coating,” Pigment Resin Technol. 53(1), 78-83. https://doi.org/10.1108/PRT-06-2022-0078

Kästner, U. (2001). “The impact of rheological modifiers on water-borne coatings,” Colloids Surf. A – Physicochem. Eng. Aspects 183, 805-821. https://doi.org/10.1016/S0927-7757(01)00507-6

Keddie, J. L. (1997). “Film formation of latex,” Materials Science and Engineering: R: Reports 21(3), 101-170. https://doi.org/10.1016/S0927-796X(97)00011-9

Keskin, H., and Tekin, A. (2011). “Abrasion resistances of cellulosic, synthetic, polyurethane, waterborne and acidhardening varnishes used woods,” Construc. Building Mater. 25(2), 638-643. https://doi.org/10.1016/j.conbuildmat.2010.07.028

Khan, M. N., Clarkson, C. M., Nuruddin, M., Sharif, A., Ahmad, E., and Youngblood, J. P. (2022). “Performance of advanced waterborne wood coatings reinforced with cellulose nanocrystals,” ACS Appl. Bio Mater. 5(9), 4179-4190. https://doi.org/10.1021/acsabm.2c00383

Khanna, P. K., Singh, N., and Charan, S. (2007). “Synthesis of nano-particles of anatase-TiO2 and preparation of its optically transparent film in PVA,” Mater. Lett. 61(25), 4725-4730. https://doi.org/10.1016/j.matlet.2007.03.064

Kilic, K., and Sögütlü, C. (2020). “Determination of the gloss values of some varnishes applied on the natural aged wood,” J. Polytechnic – Politeknik Dergisi 23(4), 1423-1431. https://doi.org/10.2339/politeknik.764261

Kiliç, K., and Sögütlü, C. (2022a). “Varnish adhesion strength in natural aged wood material,” J. Polytech. Politeknik Dergisi 26(2), 847-854. https://doi.org/10.2339/politeknik.1072314

Kiliç, K., and Sögütlü, C. (2022b). “Surface hardness of three types varnish applied to fresh and naturally aged wood,” Kastamonu Univ. J. For. Faculty 22(2), 125-134. https://doi.org/10.17475/kastorman.1179043

Kiliç, K., and Sögütlü, C. (2024). “Color change analysis of wood materials treated with different varnishes: A comparative study,” Kastamonu Univ. J. For. Fac. 24(1), 59-73. https://doi.org/10.17475/kastorman.1460453

Kim, J. H., Kwon, D. J., Lim, C. S., Seo, B. K., DeVries, K. L., and Park, J. M. (2023). “Interfacial adhesion evaluation via wettability for fiber reinforced polymer composites: A review,” Composite Interfaces 30(3), 283-299. https://doi.org/10.1080/09276440.2022.2099519

Kim, S. (2010). “Control of formaldehyde and TVOC emission from wood-based flooring composites at various manufacturing processes by surface finishing,” J. Hazard. Mater. 176, 14-19. https://doi.org/10.1016/j.jhazmat.2009.03.113

Kimerling, A. S., and Bhatia, S. R. (2004). “Block copolymers as low-VOC coatings for wood: Characterization and tannin bleed resistance,” Prog. Organic Coat. 51(1), 15-26. https://doi.org/10.1016/j.porgcoat.2004.03.006

Kinoshita, S., and Yoshioka, S. (2005). “Structural colors in nature: The role of regularity and irregularity in the structure,” ChemPhysChem 6(8), 1442-1459. https://doi.org/10.1002/cphc.200500007

Kong, L. L., Xu, D. D., He, Z. X., Wang, F. Q., Gui, S. H., Fan, J. L., Pan, X. Y., Dai, X. H., Dong, X. Y., Liu, B. X., and Li, Y. (2019). “Nanocellulose-reinforced polyurethane for waterborne wood coating,” Molecules 24(17), article 3151. https://doi.org/10.3390/molecules24173151

Korobeinichev, O., Shmakov, A., Paletsky, A., Trubachev, S., Shaklein, A., Karpov, A., Sosnin, E., Kostritsa, S., Kumar, A., and Shvartsberg, V. (2022). “Mechanisms of the action of fire-retardants on reducing the flammability of certain classes of polymers and glass-reinforced plastics based on the study of their combustion,” Polymers 14(21), article 4523. https://doi.org/10.3390/polym14214523

Korpela, A., Lillqvist, K., Rautkari, L., Rohumaa, A., Lohtander-Piispa, T., and Orelma, H. (2026). “Gaseous ozone treatment of wood: Effect of treatment conditions on the wood wettability and phenol-formaldehyde adhesive bonding strength,” BioResources 21(1), 851-860. https://doi.org/10.15376/biores.21.1.851-860

Kristak, L., Antov, P., Bekhta, P., Lubis, M. A. R., Iswanto, A. H., Reh, R., Sedliacik, J., Savov, V., Taghiyari, H. R., and Papadopoulos, A. N. (2023). “Recent progress in ultra-low formaldehyde emitting adhesive systems and formaldehyde scavengers in wood-based panels: A review,” Wood Mater. Sci. Eng. 18(2), 763-782. https://doi.org/10.1080/17480272.2022.2056080

Krongauz, V. V. (2021). “Kinetics and mechanism of plasticized poly(vinyl chloride) films autohesion interface effect,” J. Thermal Anal. Calorim. 147(6), 4177-4195. https://doi.org/10.1007/s10973-021-10832-0

Kropat, M., Hubbe, M. A., and Laleicke, F. (2020). “Natural, accelerated, and simulated weathering of wood: A review,” BioResources 15(4), 9998-10062. https://doi.org/10.15376/biores.15.4.Kropat

Kubelka, P., and Munk, F. (1931). “An article on optics of paint layers,” Z. Tech. Phys. 12(593-601), 259-274.

Kucuktuvek, M., Toker, H., Turkoglu, T., Gunduz, A., Altay, C., and Baysal, E. (2020). “Improving weathering performance of wood by borates impregnation and liquid glass coating,” Drvna Industrija 71(4), 347-354. https://doi.org/10.5552/drvind.2020.1923

Kúdela, J., Kubovský, I., Andrejko, M., and Reinprecht, L. (2021). “The impact of a CO₂ laser on the adhesion and mold resistance of a synthetic polymer layer on a wood surface,” Forests 12(2), article 242. https://doi.org/10.3390/f12020242

Kudela, J., Sikora, A., and Gondas, L. (2023). “Wood surface finishing with transparent lacquers intended for indoor use, and the colour resistance of these surfaces during accelerated aging,” Polymers 15(3), article 747. https://doi.org/10.3390/polym15030747

Kukowski, K., Hatton, J., Kozliak, E. I., and Kubátová, A. (2018). “The extent of tebuconazole leaching from unpainted and painted softwood,” Sci. Total Environ. 633, 1379-1385. https://doi.org/10.1016/j.scitotenv.2018.03.274

Kwon, Y. R., Park, J. H., Kim, H. C., Moon, S. K., and Kim, D. H. (2024). “Improving water resistance and mechanical properties of crosslinked waterborne polyurethane using glycidyl carbamate,” Polym. 16(19), article 2794. https://doi.org/10.3390/polym16192794

Lagana, R., Svocák, J., and Kúdela, J. (2021). “A study of the surface properties of a solid wood coating system with self-healing microcapsules,” in: 9th Hardwood Proceedings, Vol. 9 – Pt II: An Underutilized Resource – Hardwood Oriented Research, R. Nemeth, et al. (eds.), Univ. Sopron Niensis, pp. 61-67.

Laleicke, P. F., and Hubbe, M. A. (2025). “Outdoor wood finishing: A review on making wood resistant to moisture, ultraviolet light, and degradation,” BioResources 20(3), 7903-7982. https://doi.org/10.15376/biores.20.3.Laleicke

Landry, V., and Blanchet, P. (2012a). “Surface preparation of wood for application of waterborne coatings,” Forest Prod. J. 62(1), 39-45. https://doi.org/10.13073/FPJ-D-10-00011.1

Landry, V., and Blanchet, P. (2012b). “Weathering resistance of opaque PVDF-acrylic coatings applied on wood substrates,” Prog. Organic Coat. 75(4), 494-501. https://doi.org/10.1016/j.porgcoat.2012.06.004

Landry, V., Blanchet, P., Boivin, G., Bouffard, J. F., and Vlad, M. (2015). “UV-LED curing efficiency of wood coatings,” Coatings 5(4), 1019-1033. https://doi.org/10.3390/coatings5041019

Landry, V., Blanchet, P., and Cormier, L. M. (2013). “Water-based and solvent-based stains: Impact on the grain raising in yellow birch,” BioResources 8(2), 1997-2009. https://doi.org/10.15376/biores.8.2.1997-2009

Landry, V., Blanchet, P., and Riedl, B. (2010). “Mechanical and optical properties of clay-based nanocomposites coatings for wood flooring,” Prog. Organic Coat. 67(4), 381-388. https://doi.org/10.1016/j.porgcoat.2009.12.011

Larson, R. G., Van Dyk, A. K., Chatterjee, T., and Ginzburg, V. V. (2022). “Associative thickeners for waterborne paints: Structure, characterization, rheology, and modeling,” Prog. Polym. Sci. 129, article 101546. https://doi.org/10.1016/j.progpolymsci.2022.101546

Lee, S. C., Kwok, N. H., Guo, H., and Hung, W. T. (2003). “The effect of wet film thickness on VOC emissions from a finishing varnish,” Sci. Total Environ. 302, 75-84. https://doi.org/10.1016/S0048-9697(02)00340-6

Levinson, R., Chen, S., Slack, J., Goudey, H., Harima, T., and Berdahl, P. (2020). “Design, characterization, and fabrication of solar-retroreflective cool-wall materials,” Solar Energy Mater. Solar Cells 206, article 110117. https://doi.org/10.1016/j.solmat.2019.110117

Li, Q. S., Zhang, Y. F., Shi, L., Qiu, H. H., Zhang, S. M., Qi, N., Hu, J. C., Yuan, W., Zhang, X. H., and Zhang, K. Q. 2018). “Additive mixing and conformal coating of noniridescent structural colors with robust mechanical properties fabricated by atomization deposition,” ACS Nano 12(4), 3095-3102. https://doi.org/10.1021/acsnano.7b08259

Li, R. C., Ye, C. W., Chen, Y. T., Cao, J. Y., Qing, J. X., Liu, J. C., Xie, Z. B., and Ao, F. (2026). “Removal of alkyd resin coatings from stone heritage using an ethyl lactate-based solvent with reduced environmental impact: Multi-scale analysis and diffusion-swelling mechanism study,“ Contruc. Build. Mater. 538, article 147314. https://doi.org/10.1016/j.conbuildmat.2026.147314

Li, X. H., Chen, Y. H., Du, C. X., Liao, X. J., Yang, Y. Z., and Feng, W. (2024). “Cholesteric liquid crystal elastomer coatings with brilliant structural colors and mechanochromic response fabricated by spray deposition,” Advan. Func. Mater. 35(2), article adfm.202412298. https://doi.org/10.1002/adfm.202412298

Liang, H., Yang, P. Y., Wang, W. Z., Liu, Y. F., Ge, X. Y., and Tong, B. H. (2023). “Spreading behavior of single oil droplet impacting surface with/without a thin liquid film,” Lubricants 11(1), article 31. https://doi.org/10.3390/lubricants11010031

Lindstrand, M. (2005). “Instrumental gloss characterization – In the light of visual evaluation: A review,” J. Imaging Sci. Technol. 49(1), 61-70. https://doi.org/10.2352/J.ImagingSci.Technol.2005.49.1.art00009

Liu, J. L., and Fischer, E. C. (2023). “Review of the charring rates of different timber species,” Fire Mater. 48(1), 3-15. https://doi.org/10.1002/fam.3173

Liu, Q. Q., Gao, D., and Xu, W. (2021). “Effect of paint process on the performance of modified poplar wood antique,” Coatings 11(10), article 1174. https://doi.org/10.3390/coatings11101174

Liu, Q. Q., Gao, D., and Xu, W. (2022). “Effect of polyurethane non-transparent coating process on paint film performance applied on modified poplar,” Coatings 12(1), article 39. https://doi.org/10.3390/coatings12010039

Lokhande, G., Chambhare, S., and Jagtap, R. (2017). “Synthesis and properties of phosphate-based diacrylate reactive diluent applied to UV-curable flame-retardant wood coating,” J. Coating Technol. Res. 14(1), 255-266. https://doi.org/10.1007/s11998-016-9849-6

Lu, J. Z., Wu, Q. L., and McNabb, H. S. (2000). “Chemical coupling in wood fiber and polymer composites: A review of coupling agents and treatments,” Wood Fiber Sci. 32(1), 88-104.

Ma, Q. Z., Yu, C. Q., Zhou, Y. R., Hu, D. G., Chen, J. B., and Zhang, X. J. (2024). “A review on the calculation and application of lignin Hansen solubility parameters,” Int. J. Biol. Macromol. 256(2), article 128506. https://doi.org/10.1016/j.ijbiomac.2023.128506

Mahajan, D., Srivats, D. S., and More, A. (2023). “Synthesis of vanillin-based UV curable polyurethane dispersions for wood coating applications,” J. Coatings Technol. Res. 20, 1773-1788. https://doi.org/10.1007/s11998-023-00780-9

Mai, J. L., Yang, W. W., Zeng, Y., Guan, Y. F., and Chen, S. J. (2024). “Volatile organic compounds (VOCs) in residential indoor air during interior finish period: Sources, variations, and health risks,” Hygiene and Environmental Health Advances 9, article 100087. https://doi.org/10.1016/j.heha.2023.100087

McCrillis, R. C., Howard, E. M., Guo, Z. S., Krebs, K. A., Fortmann, R., and Lao, H. C. (1999). “Characterization of curing emissions from conversion varnishes,” J. Air Waste Manag. Assoc. 49(1), 70-75. https://doi.org/10.1080/10473289.1999.10463777

Mendes, T. J., Gonalez, J. C., Teles, R. F., and Lima, C. M. (2016). “Effect of artificial weathering on wood laminates color treated with two finishing products,” Cerne 22(1), 101-109. https://doi.org/10.1590/01047760201622011911

Mensah, R. A., Jiang, L., Renner, J. S., and Xu, Q. (2023). “Characterisation of the fire behaviour of wood: From pyrolysis to fire retardant mechanisms,” J. Thermal Anal. Calorim. 148(4), 1407-1422. https://doi.org/10.1007/s10973-022-11442-0

Miao, C. W., and Hamad, W. Y. (2019). “Critical insights into the reinforcement potential of cellulose nanocrystals in polymer nanocomposites,” Curr. Opin. Solid State Mater. Sci. 23(4), article 100761. https://doi.org/10.1016/j.cossms.2019.06.005

Mihaila, A., Danu, M., Ibanescu, C., Anghel, I., Sofran, I. E., Balanescu, L. V., Tudorachi, N., and Lisa, G. (2022). “Thermal characterization and rheological behavior of some varnishes and paints used for wood protection,” Int. J. Environ. Sci. Technol. 19(7), 6299-6314. https://doi.org/10.1007/s13762-021-03579-6

Miklecic, J., and Jirous-Rajkovic, V. (2021). “Effectiveness of finishes in protecting wood from liquid water and water vapor,” J. Building Eng. 43, article 102621. https://doi.org/10.1016/j.jobe.2021.102621

Miklecic, J., Turkulin, H., and Jirous-Rajkovic, V. (2017). “Weathering performance of surface of thermally modified wood finished with nanoparticles-modified waterborne polyacrylate coatings,” Appl. Surf. Sci. 408, 103-109. DOI: 10.1016/j.apsusc.2017.03.011

Montazeri, M., and Eckelman, M. J. (2018). “Life cycle assessment of UV-curable bio-based wood flooring coatings,” J. Cleaner Prod. 192, 932-939. https://doi.org/10.1016/j.jclepro.2018.04.209

Moorhead, D. L., and Callaghan, T. (1994). “Effects of increasing ultraviolet-B Radiation on decomposition and soil organic-matter dynamics – A synthesis and modeling study,” Biol. Fertility Soils 18(1), 19-26. https://doi.org/10.1007/BF00336439

Morris, J. (2017). “Recycle, bury, or burn wood waste biomass? LCA answer depends on carbon accounting, emissions controls, displaced fuels, and impact costs,” J. Indust. Ecol. 21(4), 844-856. https://doi.org/10.1111/jiec.12469

Mudri, N. H., Abdullah, L. C., Aung, M. M., Salleh, M. Z., Biak, D. R. A., and Rayung, M. (2020). “Comparative study of aromatic and cycloaliphatic isocyanate effects on physico-chemical properties of bio-based polyurethane acrylate coatings,” Polymers 12(7), article 1494. https://doi.org/10.3390/polym12071494

Nakamura, M. (2012). “Appearance of wood and wooden interior,” Mokuzai Gakkaishi 58(1), 1-10. https://doi.org/10.2488/jwrs.58.1

Nakanishi, E. Y., Poulin, P., Blanchet, P., Dubuis, M. E., Drouin, M., Rheaume, C., and Goupil-Sormany, I. (2024). “A systematic review of the implications of construction materials on occupants’ physical and psychological health,” Build. Environ. 257, article 111527. https://doi.org/10.1016/j.buildenv.2024.111527

Nazarenko, Y., and Narayanan, C. (2025). “Energy recovery ventilation: What is needed to fill the research gaps related to its effects on exposure to indoor bio-aerosols, nanoparticulate, and gaseous indoor air pollution,” Atmosphere 16(3), article 309. https://doi.org/10.3390/atmos16030309

Niskanen, I., Lauri, J., Yokota, M., Heikkilä, R., Hashimoto, T., and Fabritius, T. (2021). “Determination of the refractive index of particles through the immersion solid matching method,” IEEE Trans. Intrument. Meas. 70, article 6000505. https://doi.org/10.1109/TIM.2020.3016070

Nussbaum, R. M. (1999). “Natural surface inactivation of Scots pine and Norway spruce evaluated by contact angle measurements,” Holz Roh- Werkst. 57(6), 419-424. https://doi.org/10.1007/s001070050067

Özder, C., and Atar, M. (2023). “The effects of some antibacterial nano materials on varnish hardness,” J. Polytech. Politek. Dergisi 26(4), article 1325355. https://doi.org/10.2339/politeknik.1325355

Paquet, C., Brown, S., Klemberg-Sapieha, J. E., Morin, J. F., and Landry, V. (2021). “Self-healing UV-curable acrylate coatings for wood finishing system, Part 2: Impact of monomer structure and self-healing parameters on self-healing efficiency,” Coatings 11(11), article 1328. https://doi.org/10.3390/coatings11111328

Paulsson, M., and Parkås, J. (2012). “Review: Light-induced yellowing of lignocellulosic pulps – Mechanisms and preventative methods,” BioResources 7(4), 5995-6040. https://doi.org/10.15376/biores.7.4.5995-6040

Pelletier, C., Rogaume, Y., Dieckhoff, L., Bardeau, G., Pons, M. N., and Dufour, A. (2019). “Effect of combustion technology and biogenic CO2 impact factor on global warming potential of wood-to-heat chains,” Appl. Energy 235, 1381-1388. https://doi.org/10.1016/j.apenergy.2018.11.060

Phaodee, P., and Weston, J. (2023). “Review: Implementing the hydrophilic-lipophilic deviation model when formulating detergents and other surfactant-related applications,” J. Surfatants Degerg. 26(3), 277-286. https://doi.org/10.1002/jsde.12660

Poirier, G., Demers, C. M. H., and Potvin, A. (2019). “Wood perception in daylit interior spaces: An experimental study using scale models and questionnaires,” BioResources 14(1), 1941-1968. https://doi.org/10.15376/biores.14.1.1941-1968

Qian, D. F., Li, Y. G., Zhang, Q. H., Shi, G. Y., and Wang, H. Z. (2011). “Anatase TiO2 sols derived from peroxotitanium acid and to form transparent TiO2 compact film for dye-sensitized solar cells,” J. Alloys Compounds 509(41), 10121-10126. https://doi.org/10.1016/j.jallcom.2011.08.055

Ramanakoto, M. F., Andrianantenaina, A. N., Ramananantoandro, T., and Eyma, F. (2017). “Visual and visuo-tactile preferences of Malagasy consumers for machined wood surfaces for furniture: Acceptability thresholds for surface parameters,” Eur. J. Wood Wood Prod. 75(5), 825-837. https://doi.org/10.1007/s00107-016-1098-y

Ribeiro, W. C. O., Lobosco, V., and Martinez, P. F. M. (2020). “Solubility parameters analysis of Eucalyptus urograndis kraft lignin,” BioResources 15(4), 8577-8600. https://doi.org/10.15376/biores.15.4.8577-8600

Riedl, B., Angel, C., Prégent, J., Blanchet, P., and Stafford, L. (2014). “Effect of wood surface modification by atmospheric-pressure plasma on waterborne coating adhesion,” BioResources 9(3), 4908-4923. https://doi.org/10.15376/biores.9.3.4908-4923

Rosu, D., Mustata, F. R., Rosu, L., and Varganici, C. D. (2021). “Photochemical aging of eco-friendly wood coatings derived from vegetable oils,” ACS Appl. Polym. Mater. 3(12), 6303-6314. https://doi.org/10.1021/acsapm.1c01086

Royall, C. P., and Donald, A. M. (2002). “Surface properties and structural collapse of silica in matte water-based lacquers,” Langmuir 18(24), 9519-9526. https://doi.org/10.1021/la025776n

Ruwoldt, J., Tanase-Opedal, M., and Syverud, K. (2022). “Ultraviolet spectrophotometry of lignin revisited: Exploring solvents with low harmfulness, lignin purity, Hansen solubility parameter, and determination of phenolic hydroxyl groups,” ACS Omega 7(50), 46371-46383. https://doi.org/10.1021/acsomega.2c04982

Salata, R. R., Pellegrene, B., and Soucek, M. D. (2020). “Visible light cure packages for improved drying kinetics in alkyd coatings,” Prog. Organic Coatings 144, article 105672. https://doi.org/10.1016/j.porgcoat.2020.105672

Salleh, N. G. N., Alias, M. S., Gläsel, H. J., and Mehnert, R. (2013). “High performance radiation curable hybrid coatings,” Radiation Phys. Chem. 84, 70-73. https://doi.org/10.1016/j.radphyschem.2012.06.042

Salthammer, T. (2019). “Formaldehyde sources, formaldehyde concentrations and air exchange rates in European housings,” Build. Environ. 150, 219-232. https://doi.org/10.1016/j.buildenv.2018.12.042

Sang, R. J., Yang, S. Q., and Fan, Z. X. (2023a). “Effects of MDF substrate surface coating process on UV inkjet print quality,” Coatings 13(5), article 970. https://doi.org/10.3390/coatings13050970

Sang, R. J., Yang, F., and Fan, Z. X. (2023b). “The effect of water-based primer pretreatment on the performance of water-based inkjet coatings on wood surfaces,” Coatings 13(9), article 1649. https://doi.org/10.3390/coatings13091649

Sauerbier, P., Mayer, A. K., Emmerich, L., and Militz, H. (2020). “Fire retardant treatment of wood – State of the art and future perspectives,” in: Wood Fire Safety, WFS 2020, L. Makovicka Osvaldova, F. Markert, and S. Zelinka (eds), Springer, Cham., pp. 97-102. https://doi.org/10.1007/978-3-030-41235-7_14

Schmitt, J. M., and Kumar, G. (1998). “Optical scattering properties of soft tissue: A discrete particle model,” Appl. Optics 37(13), 2788-2797. https://doi.org/10.1364/AO.37.002788

Scrinzi, E., Rossi, S., Deflorian, F., and Zanella, C. (2011). “Evaluation of aesthetic durability of waterborne polyurethane coatings applied on wood for interior applications,” Prog. Organic Coatings 72(1-2), 81-87. https://doi.org/10.1016/j.porgcoat.2011.03.013

Sellman, F. A., Benselfelt, T., Larsson, P. T., and Wågberg, L. (2023). “Hornification of cellulose-rich materials – A kinetically trapped state,” Carbohyd. Polym. 318, article 121132. https://doi.org/10.1016/j.carbpol.2023.121132

Sharma, A., Tyagi, V. V., Chen, C. R., and Buddhi, D. (2009). “Review on thermal energy storage with phase change materials and applications,” Renew. Sustain. Energy Rev. 13(2), 318-345. https://doi.org/10.1016/j.rser.2007.10.005

Sherzad, M., and Jung, C. (2022). “Evaluating the emission of VOCs and HCHO from furniture based on the surface finish methods and retention periods,” Front. Built Environ. 8, article 1062255. https://doi.org/10.3389/fbuil.2022.1062255

Shi, Q., Wong, S. C., Ye, W., Hou, J. W., Zhao, J., and Yin, J. H. (2012). “Mechanism of adhesion between polymer fibers at nanoscale contacts,” Langmuir 28(10), 4663-4671. https://doi.org/10.1021/la204633c

Shukla, S., Pandey, K. K., and Kishan Kumar, V. S. (2019). “Chemical and application properties of some solvent and water based coatings on wooden substrate,” Drvna Industrija 70(2), 107-114. https://doi.org/10.5552/drvind.2019.1809

Shuyten, H. A., Weaver, J. W., and Reid, J. D. (1954), in: Fire Retardant Paints, M. W. Westgate (ed.), American Chemical Society, Washington, DC, USA, pp. 7-20. https://doi.org/10.1021/ba-1954-0009.ch003

Sigrist Photometer (no date), https://www.sigrist.com/en/GlossaryEntry/Particle-size/

Slabejová, G., Smidriaková, M., and Fekiac, J. (2016). “Gloss of transparent coating on beech wood surface,” Acta Facultatis Xylologiae Zvolen 58(2), 37-44. https://doi.org/10.17423/afx.2016.58.2.04

Slabejová, G., Smidriaková, M., and Pánis, D. (2018). “Quality of silicone coating on the veneer surfaces,” BioResources 13(1), 776-788. https://doi.org/10.15376/biores.13.1.776-788

Slabejová, G., Vidholdová, Z., and Smidriaková, M. (2023). “Change in the colour of transparent surface finish on hydrothermally treated wood,” Acta Facultatis Xylologiae Zvolen 65(1), 45-56. https://doi.org/10.17423/afx.2023.65.1.04

Smith, J. H., and Woodhouse, J. (2000). “The tribology of rosin,” J. Mechanics Phys. Solids 48(8), 1633-1681. https://doi.org/10.1016/S0022-5096(99)00067-8

Sögütlü, C., Nzokou, P., Koc, I., Tutgun, R., and Döngel, N. (2016). “The effects of surface roughness on varnish adhesion strength of wood materials,” J. Coatings Technol. Res. 13(5), 863-870. https://doi.org/10.1007/s11998-016-9805-5

Solt, P., Konnerth, J., Gindl-Altmutter, W., Kantner, W., Moser, J., Mitter, R., and van Herwijnen, H. W. G. (2019). “Technological performance of formaldehyde-free adhesive alternatives for particleboard industry,” Int. J. Adhes. Adhes. 94, 99-131. https://doi.org/10.1016/j.ijadhadh.2019.04.007

Song, S. S., and Zhao, G. J. (2011). “Psychological and emotional reactions to anatomical patterns in wood,” Wood Res. 56(4), 455-465.

Song, X. X., Guo, W. X., Zhu, Z. P., Han, G. P., and Cheng, W. L. (2024). “Preparation of uniform lignin/titanium dioxide nanoparticles by confined assembly: A multifunctional nanofiller for a waterborne polyurethane wood coating,” Int. J. Biol. Macromol. 258(1), article 128827. https://doi.org/10.1016/j.ijbiomac.2023.128827

Song, X., Wei, J., Mao, Z., Chi, X., Zhu, Z., Han, G., and Cheng, W. (2023). “Effect of hot-air drying conditions on the drying efficiency and performance of a waterborne coating on pine wood,” Forests 14(9), article 1752. https://doi.org/10.3390/f14091752

Sönmez, A., Budakçı, and M. Bayram. (2009). “Effect of wood moisture content on adhesion of varnish coatings,” Scientific Research and Essay 4 (12), 1432-1437.

Sönmez, A., Budakçi, M., Demirci, Z., and Akkus, M. (2011a). “Effects of thermal aging on the film hardness of some wood varnishes,” BioResources 6(4), 4594-4605. https://doi.org/10.15376/biores.6.4.4594-4605

Sönmez, A., Budakçi, M., and Pelit, H. (2011b). “The effect of the moisture content of wood on the layer performance of water-borne varnishes,” BioResources 6(3), 3166-3177. https://doi.org/10.15376/biores.6.3.3166-3177

Sow, C., Riedl, B., and Blanchet, P. (2011). “UV-waterborne polyurethane-acrylate nanocomposite coatings containing alumina and silica nanoparticles for wood: Mechanical, optical, and thermal properties assessment,” J. Coatings Technol. Res. 8(2), 211-221. https://doi.org/10.1007/s11998-010-9298-6

Stehr, M., and Johansson, I. (2000). “Weak boundary layers on wood surfaces,” J. Adhes. Sci. Technol. 14(10), 1211-1224. https://doi.org/10.1163/156856100742168

Sun, S. T., Wang, H., Huang, D., Ding, Y. L., Zhang, Y., Song, D. P., Zhang, K. Y., Pan, L., and Li, Y. S. (2020). “Refractive index engineering as a novel strategy toward highly transparent and tough sustainable polymer blends,” Chinese J. Polym. Sci. 38(12), 1335-1344. https://doi.org/10.1007/s10118-020-2439-1

Swartz, A. J., Curry-Nkansah, M. E., Lauer, R. P., and Gebhard, M. S. (1999). “Wood coating compositions,” US Patent 5922410 A.

Swarup, S., and Schoff, C. K. (1993). “A survey of surfactants in coatings technology,” Prog. Organic Coatings 23(1), 1-22. https://doi.org/10.1016/0033-0655(93)80002-R

Taber Industries (no date). “Taber Abraser (Abrader), The TABER® Rotary Platford Abrasion Tester – Model 1700/1750, accessed January 2026, https://www.taberindustries.com/taber-rotary-abraser

Tagg, A. S., and do Sul, J. A. I. (2019). “Is this your glitter? An overlooked but potentially environmentally-valuable microplastic,” Marine Pollut. Bull. 146, 50-53. https://doi.org/10.1016/j.marpolbul.2019.05.068

Tamantini, S., Bergamasco, S., Zikeli, F., Humar, M., Cavalera, M., and Romagnoli, M. (2023). “Cellulose nano crystals (CNC) as additive for a bio-based waterborne acrylic wood coating: Decay, artificial weathering, physical and chemical tests,” Nanomater. 13(3), article 442. https://doi.org/10.3390/nano13030442

Tao, X., Tian, D. X., Liang, S. Q., Li, S. M., Peng, L. M., and Fu, F. (2024). “Enhanced paint adhesion of puffed wood-based metal composites via surface treatment with silane coupling agent,” Wood Mater. Sci. Eng. 19(3), 573-579. https://doi.org/10.1080/17480272.2023.2269414

Thomas, F., Chen, N., Lee, I., Ford, L., Blowers, P., and Masel, R. I. (1999). “Ultraviolet high resolution electron energy loss spectroscopy of CO on Pt(110) and benzene on Pt(110),” J. Vacuum Sci. Technol. A – Vac. Surf. Films 17(4), 2339-2344. https://doi.org/10.1116/1.581770

Thorum, A. J., Allred, D. D., Pitt, W. G., and Munro, T. R. (2023). “Tuning the index of refraction of a polyvinyl toluene and polystyrene copolymer toward a heterogenous, index-matched neutron detector,” J. Appl. Polymer Sci. 140(2), article 53305. https://doi.org/10.1002/app.53305

Tian, D., Baker, D. P., and Wilson, B. L. (2021). “Wood substrate including an abrasion resistant coating,” US Patent 11033931 B2.

Tichy, R. J. (1997). Interior Wood Finishing: Industrial Use Guide, Forest Products Society, Madison, WI.

Toker, H., Baysal, E., and Kesik, H. I. (2009). “Surface characteristics of wood pre-impregnated with borates before varnish coating,” For. Prod. J. 59(7-8), 43-46.

Torcatoru, M. J., and Timar, M. C. (2024). “Light-induced colour changes in wood surfaces in indoor conditions determined by an artificial accelerated test: Influence of wood species and coating materials,” Appl. Sci. – Basel 14(3), article 1226. https://doi.org/10.3390/app14031226

Türkoglu, T., Baysal, E., Altay, Ç., Toker, H., Küçüktüvek, M., and Gündüz, A. (2020). “Investigating the surface performance of impregnated and varnished Calabrian pine wood against weathering (Gunduz, Ahmet),” Polimeros – Ciencia e Technol. 30(4), article e2020045. https://doi.org/10.1590/0104-1428.10120

Ulker, O. C., Ulker, O., and Hiziroglu, S. (2021). “Volatile organic compounds (VOCs) emitted from coated furniture units,” Coatings 11(7), article 806. https://doi.org/10.3390/coatings11070806

Vardanyan, V., Galstian, T., and Riedl, B. (2015). “Effect of addition of cellulose nanocrystals to wood coatings on color changes and surface roughness due to accelerated weathering,” J. Coatings Technol. Res. 12(2), 247-258. https://doi.org/10.1007/s11998-014-9634-3

Vardanyan, V., Poaty, B., Chauve, G., Landry, V., Galstian, T., and Riedl, B. (2014). “Mechanical properties of UV-waterborne varnishes reinforced by cellulose nanocrystals,” J. Coatings Technol. Res. 11(6), 841-852. https://doi.org/10.1007/s11998-014-9598-3

Verduyn, A., De Myer E., Torfs, J., and Van der Heijen, S. (2026). “Wood coating compositions,” US Patent 1264249 B2.

Veronovski, N., Verhovsek, D., and Godnjavec, J. (2013). “The influence of surface-treated nano-TiO2 (rutile) incorporation in water-based acrylic coatings on wood protection,” Wood Sci. Technol. 47(2), 317-328. https://doi.org/10.1007/s00226-012-0498-3

Veigel, S., Grüll, G., Pinkl, S., Obersriebnig, M., Müller, U., and Gindl-Altmutter, W. (2014). “Improving the mechanical resistance of waterborne wood coatings by adding cellulose nanofibres,” Reactive Func. Polym. 85, 214-220. https://doi.org/10.1016/j.reactfunctpolym.2014.07.020

Vidholdová, Z., and Slabejová, G. (2021). “Colour stabilisation of surface of four thermally modified woods with saturated water vapour by finishes,” Polymers 13(19), article 3373. https://doi.org/10.3390/polym13193373

Vlad-Cristea, M., Riedl, B., Blanchet, P., and Jimenez-Pique, E. (2012). “Nanocharacterization techniques for investigating the durability of wood coatings,” Eur. Polym. J. 48(3), 441-453. https://doi.org/10.1016/j.eurpolymj.2011.12.002

Wan, Q., Li, X. H., Zhang, Y. C., Song, S. S., and Ke, Q. (2021). “Visual perception of different wood surfaces: An event-related potentials study,” Anals For. Sci. 78(2), article 25. https://doi.org/10.1007/s13595-021-01026-7

Wang, J. H., and Pan, D. Y. (2025). “Microstructure and rheology of rim-charged platelike particle suspensions: A numerical study,” J. Rheol. 69(3), 267-280. https://doi.org/10.1122/8.0000899

Wang, K. L., Dong, Y. M., Ling, Z., Liu, X. R., Shi, S. Q., and Li, J. Z. (2021). “Transparent wood developed by introducing epoxy vitrimers into a delignified wood template,” Composite Sci. Technol. 207, article 108690. https://doi.org/10.1016/j.compscitech.2021.108690

Wang, Q. F., Shen, J., Shen, X. W., and Du, J. H. (2018). “Volatile organic compounds and odor emissions from alkyd resin enamel-coated particleboard,” BioResources 13(3), 6837-6849. https://doi.org/10.15376/biores.13.3.6837-6849

Wang, W. D., Shen, J., Xu, W., Liu, M., Wang, H. Y., Chen, Y., and Du, A. L. (2022a). “Characterization and analysis of very volatile organic compounds and odors from medium density fiberboard coated with different lacquers using gas chromatography coupled with mass spectrometry and olfactometry,” Wood Fiber Sci. 54(3), 196-211. https://doi.org/10.22382/wfs-2022-19

Wang, W. D., Shen, X. W., Zhang, S. Q., Lv, R. X., Liu, M., Xu, W., Chen, Y., and Wang, H. Y. (2022b). “Research on very volatile organic compounds and odors from veneered medium density fiberboard coated with water-based lacquers,” Molecules 27(11), article 3626. https://doi.org/10.3390/molecules27113626

Wang, X. H., Wei, X. Y., Liang, Y., Peng, Y. Y., Chen, S. Y., and Niu, X. T. (2025). “Advances and perspectives in natural wax composite coatings on wood-based materials: Mechanisms and applications,” Mater Today Commun. 42, article 111377. https://doi.org/10.1016/j.mtcomm.2024.111377

Wang, Y., De Assis, T., Zambrano, F., Pal, L., Venditti, R., Dasmohapatra, S., Pawlak, J., and Gonzalez, R. (2019). “Relationship between human perception of softness and instrument measurements,” BioResources 14(1), 780-795. https://doi.org/10.15376/biores.14.1.780-795

Waring, R. G. (1963). Modern Wood Finishing, Bruce Pub. Co., Milwaukee.

Weththimuni, M. L., Milanese, C., Licchelli, M., and Malagodi, M. (2021). “Improving the protective properties of shellac-based varnishes by functionalized nanoparticles,” Coatings 11(4), article 419. https://doi.org/10.3390/coatings11040419

Wieslander, G., Norback, D., Bjornsson, E., Janson, C., and Boman, G. (1997). “Asthma and the indoor environment: The significance of emission of formaldehyde and volatile organic compounds from newly painted indoor surfaces,” Int. Archives Occup. Environ. Health 69(2), 115-124. https://doi.org/10.1007/s004200050125

Williams, R. S., Knaebe, M. T., and Feist, W. C. (1996). Finishes for Exterior Wood: Selection, Application, and Maintenance: A Comprehensive Guide to the Painting/Staining and Maintenance of Homes, Decks, Log Structures, and More, Forest Products Society, Madison, WI.

Wright, N. C., Li, J. C., and Guo, M. R. (2006). “Microstructural and mold resistant properties of environment-friendly oil-modified polyurethane based wood-finish products containing polymerized whey proteins,” J. Appl. Polym. Sci. 100(5), 3519-3530. https://doi.org/10.1002/app.22432

Wu, S., Lu, Z.-L., and Zhou, Y. (2026). “Two-component aqueous sealing primer for wood substrate, sealing coating formed thereof and article,” US Patent 12577424 B2.

Wu, Y., Liu, G. J., Li, H., Han, P. S., Cheng, J. Y., and Zhou, L. (2020c). “Preparation and application of photonic crystal paints with tunable structural colors,” Physica Status Solidi A – Appl Mater. Sci. 217(9), article 1900539. https://doi.org/10.1002/pssa.201900539

Wu, Y., Wu, J. M., Wang, S. Q., Feng, X. H., Chen, H., Tang, Q. W., and Zhang, H. Q. (2019). “Measurement of mechanical properties of multilayer waterborne coatings on wood by nanoindentation,” Holzforschung 73(9), 871-877. https://doi.org/10.1515/hf-2018-0193

Wu, Y., Wu, X. Y., Yang, F., Zhang, H. Q., Feng, X. H., and Zhang, J. L. (2020a). “Effect of thermal modification on the nano-mechanical properties of the wood cell wall and waterborne polyacrylic coating,” Forests 11(12), article 1247. https://doi.org/10.3390/f11121247

Wu, Y., Zhang, H. Q., Yang, L. C., Wang, S. Q., and Meng, Y. J. (2020b). “Understanding the effect of extractives on the mechanical properties of the waterborne coating on wood surface by nanoindentation 3D mapping,” J. Mater. Sci. 56(2), 1401-1412. https://doi.org/10.1007/s10853-020-05347-2

Xie, R., and Xing, D. (2026). “Development and application of ultraviolet shielding materials in the field of wood protection: A review,” European Journal of Wood and Wood Products 84(4), 100. https://doi.org/10.1007/s00107-026-02455-9

Xu, D. D., Liang, G. T., Qi, Y. R., Gong, R. Z., Zhang, X. Q., Zhang, Y. M., Liu, B. X., Kong, L. L., Dong, X. Y., and Li, Y. F. (2022). “Enhancing the mechanical properties of waterborne polyurethane paint by graphene oxide for wood products,” Polymers 14(24), article 5456. https://doi.org/10.3390/polym14245456

Xu, F., Zi, B., Wang, J., et al. (2024). “Multi-objective trajectory optimization for rigid-flexible coupling spray-painting robot integrated with coating process constraints,” Chinese Journal of Mechanical Engineering 37, article 152. https://doi.org/10.1186/s10033-024-01130-5

Yalcin, M., Pelit, H., Akcay, C., and Cakicier, N. (2017). “Surface properties of tannin-impregnated and varnished beech wood after exposure to accelerated weathering,” Coloration Technol. 133(4), 334-340. https://doi.org/10.1111/cote.12287

Yamane, C., Aoyagi, T., Ago, M., Sato, K., Okajima, K., and Takahashi, T. (2006). “Two

different surface properties of regenerated cellulose due to structural anisotropy,” Polymer J. 38(8), 819-826. https://doi.org/10.1295/polymj.PJ2005187

Yan, X. X., Chang, Y. J., and Qian, X. Y. (2019). “Effect of the concentration of pigment slurry on the film performances of waterborne wood coatings,” Coatings 9(10), article 635. https://doi.org/10.3390/coatings9100635

Yan, X. X., Li, W. B., Han, Y., and Yin, T. Y. (2022). “Preparation of melamine/rice husk powder coated shellac microcapsules and effect of different rice husk powder content in wall material on properties of wood waterborne primer,” Polymers 14(1), article 72. https://doi.org/10.3390/polym14010072

Yan, X. X., Tao, Y., and Qian, X. Y. (2020c). “Preparation and optimization of waterborne acrylic core microcapsules for waterborne wood coatings and comparison with epoxy resin core,” Polym. 12(10), article 2366. https://doi.org/10.3390/polym12102366

Yan, X. X., Wang, L., and Qian, X. Y. (2020a). “Effect of coating process on performance of reversible thermochromic waterborne coatings for Chinese fir,” Coatings 10(3), article 223. https://doi.org/10.3390/coatings10030223

Yan, X. X., Wang, L., and Qian, X. Y. (2020b). “Effect of microcapsules with different core-wall ratios on properties of waterborne primer coating for European linden,” Coating 10(9), article 826. https://doi.org/10.3390/coatings10090826

Yan, X. X., Zhao, W. T., and Wang, L. (2021). “Preparation and performance of thermochromic and self-repairing dual function paint film with lac resin microcapsules and fluorane microcapsules,” Polymers 13(18), article 3109. https://doi.org/10.3390/polym13183109

Yang, D. P., Luo, W. J., Huang, Y. D., and Huang, S. M. (2019). “Facile synthesis of monodispersed SiO2@Fe3O4 core-shell colloids for printing and three-dimensional coating with noniridescent structural colors,” ACS Omega 4(1), 528-534. https://doi.org/10.1021/acsomega.8b02987

Yang, F., Wu, Y., Zhang, S. Q., Zhang, H. M., Zhao, S. L., Zhang, J. L., and Fei, B. H. (2020). “Mechanical and thermal properties of waterborne polyurethane coating modified through one-step cellulose nanocrystals/graphene materials sols method,” Coatings 10(1), article 40. https://doi.org/10.3390/coatings10010040

Yang, L., and Kruse, B. (2004). “Revised Kubelka-Munk theory. I. Theory and application,” J. Optical Soc. Amer. 21(10), 1933-1941. https://doi.org/10.1364/JOSAA.21.001933

Yang, Q., Wang, N., Yi, L., and Yan, L. (2024). “Construction of decorative, antibacterial, anti-aging and fire-retardant integrative coatings for wood substrates with super protective performances,” Polym. Degrad. Stabil. 219, article 110620. https://doi.org/10.1016/j.polymdegradstab.2023.110620

Yang, W., and Ke, J.-H. (2022). “Aqueous coating compositions for forming anti-grain-puffing coatings on wood substrate, aqueous paints and articles,” US Patent 11535768 B2.

Yoo, Y., and Youngblood, J. P. (2017). “Tung oil wood finishes with improved weathering, durability, and scratch performance by addition of cellulose nanocrystals,” ACS Appl. Mater. Interfac. 9(29), 24936-24946. https://doi.org/10.1021/acsami.7b04931

Yuan, J. H., Jiao, Z. C., Kong, X. F., Chai, J. L., and Emura, K. (2025). “Application and development of retroreflective Materials: A review,” Energy Buildings 337, article 115707. https://doi.org/10.1016/j.enbuild.2025.115707

Yurtsever, M. (2019). “Glitters as a source of primary microplastics: An approach to environmental responsibility and ethics,” J. Agric. Environ. Ethics 32(3), 459-478. https://doi.org/10.1007/s10806-019-09785-0

Zareanshahraki, F., and Mannari, V. (2021). “Formulation and optimization of radiation-curable nonisocyanate polyurethane wood coatings by mixture experimental design,” J. Coatings Technol. Res. 18(3), 695-715. https://doi.org/10.1007/s11998-020-00453-x

Zahedi, S., Zaarei, D., and Ghaffarian, S. R. (2018). “Self-stratifying coatings: A review,” J. Coatings Tenchnol. Res. 15(1), 1-12. https://doi.org/10.1007/s11998-017-9996-4

Zhang, Y., Huang, Y. P., Li, M. C., Zhang, S., Zhou, W. M., Mei, C. T., Pan, M. Z. (2023). “Bioinspired, stable adhesive Ti3C2Tx MXene-based coatings towards fire warning, smoke suppression and VOCs removal smart wood,” Chem. Eng. J. 452(4), article 139360. https://doi.org/10.1016/j.cej.2022.139360

Zhang, Y., Guo, Y., Wei, P., He, Z., Yi, S., and Zhao, G. (2024a). “Effect of changes in surface visual properties of heat-treated wood on the psychological preference,” BioResources 19(3), 4652-4669. https://doi.org/10.15376/biores.19.3.4652-4669

Zhang, Y., Guo, Y. Y. Z., Wei, P. X., He, Z. B., Yi, S. L., and Zhao, G. J. (2024b). “Effect of changes in surface visual properties of heat-treated wood on the psychological preference,” BioResources 19(3), 4652-4669. https://doi.org/10.15376/biores.19.3.4652-4669

Zhang, H. Q., Feng, X. H., Wu, Y., Wu, Z. H. (2024c). “Self-matting waterborne poly-urethane acrylate wood coating by 222 nm far-UVC irradiation in ambient air,” Prog. Organic Coat. 189, article 018305. https://doi.org/10.1016/j.porgcoat.2024.108305

Zhang, Y., Xiong, W., Guo, Y., Wei, P., and Yi, S. (2025). “Multimodal evaluation of warmth perception in wood: An experimental study based on visual, tactile, and visual-tactile interactions,” BioResources 20(3), 7495-7514. https://doi.org/10.15376/biores.20.3.7495-7514

Zhao, G. F., Ni, H. Y., Jia, L. N., Ren, S. X., and Fang, G. Z. (2018). “Quantitative analysis of relationship between Hansen solubility parameters and properties of alkali lignin/acrylonitrile-butadiene-styrene blends,” ACS Omega 3(8), 9722-9728. https://doi.org/10.1021/acsomega.8b00954

Zhou, K. K., Xu, M. P., Wu, W. J., and Wang, J. (2023). “Preparation of nano silicon carbide modified UV paint and its application performance on wood flooring surface,” Polymers 15(23), article 4584. https://doi.org/10.3390/polym15234584

Zhu, X. D., Liu, Y., and Shen, J. (2016). “Volatile organic compounds (VOCs) emissions of wood-based panels coated with nanoparticles modified water based varnish,” Eur. J. Wood Wood Prod. 74(4), 601-607. https://doi.org/10.1007/s00107-016-1012-7

Zhu, Y. D., Zhu, W. K., Li, Z. Q., Feng, Y., Qi, W., Li, S., Wang, X. Y., and Chen, M. L. (2023). “Enhancement of wood coating properties by adding silica sol to UV-curable waterborne acrylics,” Forests 14(2), article 335. https://doi.org/10.3390/f14020335

Zobeiry, N., Lee, A., and Mobuchon, C. (2020). “Fabrication of transparent advanced composites,” Composites Sci. Technol. 197, article 108281. https://doi.org/10.1016/j.compscitech.2020.108281

Zöttl, A., Tesser, F., Matsunaga, D., Laurent, J., du Roure, O., and Lindner, A. (2023). “Asymmetric bistability of chiral particle orientation in viscous shear flows,” Proc. Nat. Acad. Sci. USA 120(45), article e2310939120. https://doi.org/10.1073/pnas.2310939120