Abstract
Selective Laser Sintering (SLS) is an advanced additive manufacturing technology that is widely used in multiple fields. This study investigated the effects of laser power and scanning speed on the SLS melt pool using FLOW-3D numerical simulations and experimental validation. The raw material was a mixture of walnut shell powder and copolyester (co-PES) hot melt adhesive powder. Experimental temperature measurements confirmed the numerical model’s accuracy, revealing a deviation of less than 10% between the simulated and actual center temperatures of the melt pool. The results demonstrated that a stable, continuous single-track melt pool was achieved under optimal parameters of 10 W laser power and 1400 mm/s scanning speed. Conversely, increasing the scanning speed to 1600 to 2200 mm/s at a constant 10 W power substantially reduced thermal energy input. This reduction induced a transition to metastable melt pools, ultimately leading to the formation of semi-melted particles. These insights can provide a basis for optimization of SLS manufacturing parameters.
Download PDF
Full Article
Laser Sintering Powder Bed Simulation: Effects of Laser Power and Scanning Speed on the Melt Pool in Selective Laser Sintering of Walnut Shell/Co-Polyester Composite
Yueqiang Yu,a,b,c Chenxiang Yuan,b Ting Jiang,b,c,* Yanling Guo,d Sheng Gao,b,c,* Guangyu Li,b Jichang Wang,b Zenan Li,b and Bakary S. Doumbia e
Selective Laser Sintering (SLS) is an advanced additive manufacturing technology that is widely used in multiple fields. This study investigated the effects of laser power and scanning speed on the SLS melt pool using FLOW-3D numerical simulations and experimental validation. The raw material was a mixture of walnut shell powder and copolyester (co-PES) hot melt adhesive powder. Experimental temperature measurements confirmed the numerical model’s accuracy, revealing a deviation of less than 10% between the simulated and actual center temperatures of the melt pool. The results demonstrated that a stable, continuous single-track melt pool was achieved under optimal parameters of 10 W laser power and 1400 mm/s scanning speed. Conversely, increasing the scanning speed to 1600 to 2200 mm/s at a constant 10 W power substantially reduced thermal energy input. This reduction induced a transition to metastable melt pools, ultimately leading to the formation of semi-melted particles. These insights can provide a basis for optimization of SLS manufacturing parameters.
DOI: 10.15376/biores.21.4.11467-11482
Keywords: Additive manufacturing; Selective laser sintering; Biomass composite; Walnut shell powder; Temperature field; Sintering appearance
Contact information: a: Key Laboratory of Advanced Manufacturing and Intelligent Technology (Ministry of Education), Harbin 150080, China; b: College of Mechanical Science and Engineering, Northeast Petroleum University, Daqing, 163318, China; c: Heilongjiang Province Petroleum Drilling and Production Equipment Remanufacturing Technology Innovation Center, Northeast Petroleum University, Daqing, 163318, China; d: Research and Development Center of 3D Printing Material and Technology Northeast Forestry University, Harbin 150040, China; e: Forestry and Woodworking Machinery Engineering Technology Center, Northeast Forestry University, Harbin 150040, China;
* Corresponding authors: [email protected]; [email protected]
INTRODUCTION
Selective Laser Sintering (SLS) is an advanced Additive Manufacturing (AM) technique specifically designed for the efficient production of metal parts with complex geometries. It works by using a high-power laser beam to precisely scan the surface of pre-heated powder material according to the 2D cross-sectional paths of a part, causing the powder particles to locally melt and fuse together into a solid layer; subsequently, the build platform becomes lowered by a single layer’s thickness, a recoater spreads a fresh layer of powder, and the laser scans and sinters again, repeating this layer-by-layer accumulation process until the complete 3D solid part is finally formed. Its working principle is shown in Fig. 1. In recent years, SLS technology has been widely applied in various industrial sectors such as aerospace (Zhang et al. 2019) and biomedicine (Kamboj et al. 2021).
With the increasing demand for sustainable manufacturing, the application of biomass and polymer composites in SLS has garnered a lot of attention. Researchers have successfully fabricated scaffolds and parts using various sustainable materials, demonstrating their processability. For instance, Salmoria et al. (2009) confirmed the printability of pure cellulose-based biopolymers, while Jonkers et al. (2021) reported the SLS forming of pure starch-based food, revealing its anisotropic mechanical behavior. In the realm of biomass composites, Zhao et al. (2015) confirmed that bamboo powder/ copolyamide composites exhibit good laser sintering characteristics. To address the poor mechanical properties of traditional wood-plastic materials, Yu et al. (2018) prepared walnut shell-based composite powders, showing that the addition of copolyamide (Co-PA) can effectively regulate the sintering characteristics. Furthermore, studies by Idriss et al. (2020) on sisal fiber/polyethersulfone and Zhang et al. (2021) on aluminum-enhanced wood-plastic composites have established empirical process–property relationships, highlighting how preheating, laser power, and scan speed affect macroscopic mechanical performance. In the field of metal selective laser sintering, some research (Amorim et al. 2014) has directly fabricated Mo-CuNi composite material electrodes using selective laser sintering technology, demonstrating that by rationally optimizing process parameters such as laser scanning speed and hatch distance, it is then possible to prepare complex functional parts with high density and excellent electrical discharge machining performance. Liu et al. (2007) studied the process of indirect SLS forming using composite element powders (CEPs), successfully manufacturing a series of high-performance metal parts such as Fe-Cu-C through laser sintering forming blanks, polymer binder thermal decomposition, and subsequent copper melt infiltration treatment.
However, despite these material innovations, a major challenge in SLS adoption involves the occurrence of defects during the manufacturing process. Unstable melt pools can substantially increase the chances of gas entrapment, porosity, and poor surface finish (Yi et al. 2016). Traditional trial-and-error methods used to optimize process parameters are not only inefficient but also costly. Consequently, there is a strong call for a deeper understanding of the intrinsic mechanisms of defect formation from a mathematical and physical perspective. Numerical simulation provides an effective solution to replicate the complex transient SLS processing procedure. In the biomass domain, Yu et al. (2021) recently utilized a double ellipsoidal heat source model to quantitatively investigate the structural morphology of the melt pool for walnut shell/co-polyester (Co-PES) composites (WSPC), providing valuable preliminary theoretical support.
While SLS has been extensively researched in the context of metallic materials, a comprehensive, systematic understanding of the molten pool dynamic evolution and defect formation mechanisms for complex biomass composites remains insufficient. Current research on biomass materials primarily emphasizes the optimization of process parameters through empirical methods or the improvement of macro-mechanical properties; the intrinsic physical mechanisms governing the transition of complex biomass/hot-melt adhesive composite systems from stable to metastable or unstable molten pool states under laser irradiation have not yet been fully elucidated.
To profoundly understand the intrinsic correlation between process parameters and forming defects, it is imperative to focus on the core thermophysical characteristics reflecting melt pool stability: the center temperature and the sintering depth. The center temperature refers to the peak temperature at the laser irradiation spot, which dictates the melting degree and fluidity of the binder. A low temperature results in insufficient melting, producing semi-melted particles and poor fusion issues; conversely, an excessively high temperature may induce thermal decomposition. The sintering depth represents the vertical penetration distance of the laser energy into the powder bed. Inadequate depth compromises interlayer bonding strength, while excessive depth can cause thermal damage to the underlying material. Both parameters play a pivotal role in controlling defect generation and ensuring part quality (Panwisawas et al. 2017).
Although the SLS technology has been widely studied in the fields of metal materials and traditional polymer materials, there is still a lack of comprehensive and systematic understanding of the dynamic evolution laws of the molten pool and the defect formation mechanisms for biomass composite materials such as walnut shell powder. The current numerical simulation studies on the temperature field of SLS mostly focus on using the homogeneous model, which simplifies the powder bed into a continuous and uniform medium and fails to effectively express the microscopic state changes of discrete powder particles under laser action, the heat conduction between particles, and the transient fluid dynamics behavior within the molten pool.
Given the limitations of the studies, this research aimed to systematically clarify the influence patterns of laser power and scanning rate on the morphology of the molten pool and temperature field changes of walnut shell/Co-PES composite powder particles during SLS process. To this end, this research utilized the FLOW-3D software to establish a dynamic numerical model at the discrete particle scale, and for the first time achieved a dynamic simulation analysis of the entire process of this biomass composite material from “powder laying, laser melting, molten pool evolution to defect generation”. This analysis deeply elucidated the intrinsic physical mechanism of the material’s transformation from a stable molten pool to an unstable or non-stable molten pool state under laser radiation. At the same time, by using the method of mutual verification between experiments and simulations, the accuracy of this discrete particle model was demonstrated, which can provide a high-precision and transferable modeling theoretical framework for the precise optimization of the process parameters of the selective laser sintering process of environmentally friendly biomass composite materials.
Fig. 1. Schematic diagram of the working principle of SLS
NUMERICAL SIMULATION AND EXPERIMENT METHODS
Physical Simulation
The physical model for the SLS process is illustrated in Fig. 2. The computation domain measures 500 μm × 1000 μm × 400 μm, with the substrate and gas region heights set at 200 μm and 80 μm, respectively. To balance numerical accuracy with computational efficiency, a hexahedral mesh with a 5-um cell size was adopted, resulting in approximately 1.8 million elements. Walnut shell powder particles with an average diameter of 100 μm and copolyester hot melt adhesive powder particles with an average diameter of 58 μm are spread on the substrate to form a powder bed with a thickness of 110 μm. The powder bed laying process is simulated using the Discrete Element Method (DEM).
Numerical simulations were performed using FLOW-3D based on the following assumptions: (1) fluid flow within the molten pool is treated as incompressible laminar flow; and (2) all thermophysical properties are temperature-dependent, with the latent heat of the composite powder varying linearly within the phase-change temperature range.
Fig. 2. Powder bed simulation model
Governing Equation
To reduce computation time, it is assumed that the fluid is incompressible. Therefore, the mass conservation equation is,
(1)
where ρ is the fluid density (kg/m3); t is time (s); u,v, and w are the velocity components (m/s) in the x,y, and z directions, respectively; VF is the volume fraction of the fluid material; and Ax, Ay, and Az are the area fractions of the fluid material in the x, y, and z directions, respectively.
The energy conservation equation is:
(2)
where is the internal energy of the mixture (J/kg) and is the temperature of the material (K).
Laser Heat Source and Laser Absorptivity
During the SLS process, the commonly used heat sources are mainly divided into surface heat sources and volumetric heat sources. The surface heat source is a simplified form of the volumetric heat source. In this study, a Gaussian surface heat source is used for the simulation. The mathematical expression is,
(3)
When the laser irradiates the surface of the powder bed, the laser energy is decomposed into absorbed energy, reflected energy, and transmitted energy. Because the wavelength of the CO2 laser is 10.6 μm, it is difficult for it to penetrate walnut shell composite powder. Therefore, the laser absorption rate is mainly determined by the absorbed energy and reflected energy. Because walnut shell composite powder contains a large amount of polymer materials, it was assumed that the absorption rate of walnut shell composite powder for CO2 lasers was approximately the same as that of polymer materials for CO2 lasers. In this study, the laser absorption rate was set to 0.95 (Yu et al. 2021).
Boundary Condition
In this study, the thermal expansion of the material has a negligible impact on its heat transfer. Non-uniform heat distribution is an important issue that leads to deformation and stress concentration. However, deformation and stress are largely influenced by solid-state phase transformations of the material, which involve highly nonlinear thermomechanical plasticity issues, complicating the model. Therefore, this study does not consider thermal stress issues. Furthermore, the solid phase density of the material is assumed to be constant.
Regarding the driving forces, gravity, surface tension, Marangoni effect, and vapor recoil pressure, are primarily considered. Surface tension is simplified as an equivalent pressure acting on the melt pool surface, which accounts for its linear relationship with temperature. The surface tension coefficient was calculated following Eq. 4,
(4)
Temperature gradients cause variations in surface tension, resulting in fluid flow, known as the Marangoni effect. In the forming process, vapor recoil force is the primary driving force:
Figure 3 presents the curves showing the thermal conductivity, specific heat capacity, and density of walnut shell/polyester hot melt adhesive powder as functions of temperature. Other parameters are kept constant as specified in Table 1.
Fig. 3. Physical property parameters vary with temperature: (a) Thermal conductivity; (b) Specific heat; (c) Density
Table 1. Thermal Properties of Walnut Shell/Polyester Hot Melt Adhesive Powder
Experiment Methods
To verify the correctness of the numerical model, experiments were conducted to validate the temperature field during SLS under varying powder spreading speeds and laser powers. Walnut shell/ Co-PES composite powder was utilized as the raw material, with the particle size distribution of walnut shell particles depicted in Fig. 4.The walnut shell / copolyester hot melt adhesive powder is mainly composed of walnut shell powder and modified copolyester hot melt adhesive powder, with the two powders accounting for more than 90% of the total mass of the composite powder. The quality ratio of walnut shell powder to copolyester hot melt adhesive powder is 1:4. To improve the fluidity and heat absorption of the composite powder, a small amount of lubricant and light stabilizer auxiliary reagents were added. The parameters of thermal conductivity, specific heat capacity and density of WSPC powder varying with temperature are shown in Table 2.
Table 2. Thermophysical Parameters of WSPC Powder
To verify the validity of the numerical model of the temperature field, selective laser sintering temperature field validation experiments were conducted under different scanning speeds and different laser powers. The experiment utilized the AFS-360SLS rapid prototyping system from Beijing Longyuan Automatic Forming System Co., Ltd. During the experiment, surface temperatures of the powder bed under various process parameters were measured using an infrared thermal camera. Experiments were conducted using laser power settings of 10 W and varying laser scanning speeds of 1.4 m/s, 1.6 m/s, 1.8 m/s, 2.0 m/s, and 2.2 m/s, as well as laser scanning speed of 2.0 m/s and varying laser powers of 8 W, 10 W, 12 W, and 14 W. Infrared thermal imager was used to record the sintering temperature during the sintering process.
Fig. 4. Particle size distribution result
RESULTS AND DISCUSSION
Effect of Scanning Speed on Sintering Channel and Temperature Field
Increasing the laser scanning speed not only enhances the manufacturing efficiency of walnut shell/polyester hot melt adhesive composite powder parts but also notably impacts the laser energy density. A higher scanning speed reduces the exposure time of the powder to laser radiation, potentially causing insufficient heating of the powder and the formation of defects, which could adversely affect the mechanical properties of the sintered parts. Table 3 displays the simulated parameters for single-track formation at various speeds in this section of the study.
Table 3. Simulation Parameters at Different Laser Scanning Speeds
Figure 5 presents the transient temperature contour maps and the morphological evolution of the sintering tracks extracted from the mesoscale powder bed numerical simulation. For each scanning speed, both the top view (a1, a3, b1, b3, c1, c3) to observe the track continuity and the longitudinal cross-sectional view along the laser scanning path (a2, a4, b2, b4, c2, c4) to observe the penetration depth and wetting behavior at different time steps were extracted. At a laser power of 10 W and a scanning speed of 1400 mm/s (Fig. 5a), the laser energy input is found to be sufficient. The Co-PES binder fully melts, resulting in low viscosity and excellent fluidity. Driven by capillary forces, the melt thoroughly wets the walnut shell particles and spreads evenly, forming a continuous and stable sintering track. The single-track melt pool stabilizes into a continuous, comet-like shape that promotes high component density. This stability is characterized by the absence of a disconnected rear transition zone and a steady depression area at the laser interaction point, where recoil pressure balances the Marangoni effect to drive counterclockwise melt circulation. The Gaussian energy distribution ensures complete melting from the center outward. Furthermore, this lower scanning speed extends the liquid dwell time, promoting thorough spreading, complete powder infiltration, and high bed density, ultimately yielding a smooth sintering track.
When the scanning speed increases to 1600 mm/s, the reduced laser heat input creates a metastable melt pool exhibiting local “bottleneck” phenomena (Fig. 5b). The faster heat source fails to completely melt densely packed large walnut shell particles, leaving voids that degrade surface roughness. At this stage, the Plateau-Rayleigh instability begins to dominate. The surface tension forces the liquid cylinder to contract locally to minimize surface energy, leading to necking phenomena and the formation of the observed “Bottleneck” regions. Conversely, areas with smaller polyester adhesive particles melt rapidly. This cyclic melting disparity destabilizes track formation. Additionally, the shallower penetration depth prevents large particles from fully bonding with the substrate, leaving gaps that compromise interlayer connectivity.
At 1800 mm/s (Fig. 5c), the thermal input decreases further and the Co-PES binder barely melts, leading to transient melt pools and severe sphericalization defects. This disrupts pool continuity, fragmenting the track into isolated heated zones and island-like regions. This sphericalization is further exacerbated by the random distribution of powder particles, Marangoni flow, gravity, and poor wetting effects.
Fig. 5. The formation process of sintering tracks at different scanning speeds when the laser power is 10 W: (a) 1400 mm/s; (b) 1600 mm/s; (c) 1800 mm/s
As shown in Fig. 5, the further reduction in laser thermal input limits the penetration depth, causing the powder layer to only partially melt. In this regime, the surface tension of the molten pool overcomes the substrate’s wetting forces, triggering a capillary instability that aggregates the melt into spherical clusters rather than promoting lateral spreading. Consequently, lack-of-fusion gaps form between the track and the substrate, which compromises subsequent layer deposition and increases surface roughness—defects that must be eliminated to ensure dimensional accuracy.
Simulations at 10 W with scanning speeds of 2000 mm/s and 2200 mm/s (Fig. 6) demonstrate that extreme scanning speeds fail to meet the melting threshold. The resulting tracks exhibit a ‘semi-melted’ state, where only the upper particle regions liquefy while the lower regions remain solid, leading to extensive unbonded gaps between the partially melted track and the underlying unmelted powder bed.
Across the velocity range examined, the thermal profile within the walnut shell/polyester powder bed remains qualitatively consistent. The temperature peaks instantaneously at the laser-interaction center, followed by asymmetric thermal diffusion toward the track boundaries and a gradual post-scanning cooling phase.
Fig. 6. The sintering path formation process with a laser power of 10 W and an increased scanning speed of 2000 mm/s (a1, a2) and 2200 mm/s (b1, b2)
Effect of Laser Power on Sintering Channel and Temperature Field
Laser power is a critical factor influencing the quality of SLS fabrication. Higher laser power translates to increased laser thermal input energy, which ensures more thorough heating of the powder and consequently higher processing costs. Conversely, lower laser power reduces the thermal input energy, potentially leading to inadequate powder heating, defects, and compromised mechanical properties in the sintered parts. Table 4 outlines the simulation parameters for single-track formation under various laser powers in this study.
Table 4. Simulation Parameters of Single Pass Forming Under Different Laser Power
Figure 7 presents single-track sintering simulations at varying laser powers. At 8 W, insufficient thermal input leaves powder particles in a semi-molten state (Fig. 7a). Increasing the power to 10 W generates a transient molten pool characterized by balling defects and irregular interfacial gaps, indicating inadequate thermal penetration and poor substrate adhesion (Fig. 7b). At 12 W, the pool transitions to a metastable state, exhibiting localized necking due to an insufficient melt driving force (Fig. 7c). Conversely, a 14 W laser power provides adequate thermal input for thorough melt infiltration into interstitial gaps, yielding a stable pool morphology, smooth tracks, and enhanced densification (Fig. 7d).
Moreover, cross-sectional morphologies (Fig. 7c) confirm that elevated laser power monotonically expands both molten pool depth and width by facilitating deeper energy penetration and lateral spreading. Thermally, the walnut shell/polyester powder bed exhibits a consistent profile across all parameters: temperatures peak rapidly at the laser center, diffuse asymmetrically toward the track edges, and cool gradually post-irradiation.
Laser power substantially influences the dimensions of melt pools. Figure 8 illustrates the cross-sectional morphology of melt pools at varying laser powers, depicted in Fig. 8(a) to (d). It is evident that increasing laser power correlates with higher thermal input energy. This enhanced energy penetration allows the laser to reach the substrate through the powder layer, providing ample force for molten material to spread. As a result, there is a noticeable increase in both the depth and width of the melt pool.
Fig. 7. Simulation of single path formation under different laser powers: (a1) (a2) 8 W; (b1) (b2) 10 W; (c1) (c2) 12 W; (d1) (d2) 14 W
Fig. 8. The effect of laser power on the melt pool’s width and depth: (a) 8 W; (b) 10 W; (c) 12 W; (d) 14 W
Experimental Validation of the Numerical Model
The measurement process of the infrared thermometer is shown in Fig. 9. The thermogravimetric curves of walnut shell powder and Co-PES powder are shown in Fig. 10a, and the DSC curves are shown in Fig. 10b.
From the TG curves, the walnut shell component contains organic components, and these organic components only start to undergo marked thermal decomposition when the temperature is much higher than 573 K. In this study, the peak temperature within the stable sintering process range was basically within the temperature range where the copolyester hot melt adhesive was completely melted. Within this processing temperature range, the TG curve shows that both the walnut shell and the composite powder maintained a very high-quality retention level, indicating that this processing window can effectively prevent walnut shell particles from experiencing excessive heating or thermal degradation. At the same time, combining the heat absorption and release characteristics of the DSC curve, the Co-PES and the composite powder exhibited a marked heat absorption peak near 320 to 340K, confirming their initial melting behavior. Under the experimental conditions used in this study, the peak temperature achievable during the stable sintering stage was much lower than the typical glass transition temperature of pure lignin. Therefore, it can be concluded that under the current processing conditions, lignin remained in a solid state and did not undergo liquefaction.
Fig. 9. Temperature data collection: (a) Optical view of the temperature measurement area; Corresponding infrared thermal image
Fig. 10. Thermal properties curves of walnut shell/Co-PES powder: (a) TG curves; (b) DSC curves
The temperature acquisition results are presented in Fig. 11. It is evident that there was a deviation of less than 10% between the simulated and actual values of the center temperature of the melt pool for walnut shell/Co-PES powder. Overall, the simulated temperature values were higher than the actual temperature values, likely influenced by factors, such as ambient temperature and air cooling, during the experiment. However, the trend of temperature variation between simulation and experiment remained consistent. This suggests that within an acceptable margin of error, the numerical model is fundamentally accurate.
Fig. 11. Temperature data collection result: (a) Scanning speed; (b) Laser power
Figure 12 presents a quantitative comparison between the numerical simulation results and the experimental measurements, focusing on both the center temperature of the melt pool (Fig. 12a) and the penetration depth (Fig. 12b). As depicted in Fig. 12a, the simulated peak temperatures align closely with the experimentally recorded values across various scanning speeds, maintaining a relative deviation of less than 10%. Although the simulated temperatures are marginally higher, likely attributable to unmodeled convective heat losses to the ambient air during physical testing, the overall decreasing trend with accelerated scanning speed is highly consistent. Similarly, Fig. 12b illustrates that both simulation and experiment demonstrate a monotonic increase in sintering depth as the laser power rises. The strong correlation between the predicted and measured data across different parameter windows confirms the high fidelity of the established FLOW-3D numerical model, justifying its reliability for further predictive analysis of the molten pool dynamics.
To further quantitatively evaluate the accuracy of the numerical model, a statistical analysis was conducted on the center temperature of the melt pool in the simulation and the experimental measurements. Under a constant laser power of 10 W, the Pearson correlation coefficient, determination coefficient R2, and root mean square error (RMSE) were calculated for five scanning speeds (1400 to 2200 mm/s). The results showed that the Pearson correlation coefficient between the simulated temperature and the experimental measurement values was 0.9987, and the determination coefficient R2 was 0.9974, indicating an excellent linear correlation between the two; the RMSE was 27.11 K, which was within the acceptable range of the inherent uncertainty of the infrared thermal imager measurement. The above quantitative statistical indicators, together with the relative deviation of less than 10%, jointly confirmed that the established FLOW-3D numerical model has a high fidelity in predicting the temperature field and dynamic evolution of the SLS of walnut shell/Co-PES composite.
Fig. 12. Comparison between simulated values and measured values of (a) temperature and (b) sintering depth
CONCLUSIONS
- Scanning speed was identified as a critical determinant of the forming quality in single-track laser sintering. A continuous, smooth, and defect-free molten pool morphology can be obtained at a laser power of 10 W and a scanning speed of 1400 mm/s; a deeper molten pool penetration and good interlayer bonding can be achieved at a laser power of 18 W and a scanning speed of 1800 mm/s.
- The elevation of laser power substantially enhances the thermal input energy, acting as a primary driver for the dynamic evolution and macroscopic dimensions of the melt pool. Experimental and simulation results demonstrate that the width and depth of the molten pool expand monotonically with increasing laser power, which is attributed to deeper energy penetration and enhanced lateral spreading.
- This study established a validated FLOW-3D numerical framework that, for the first time, systematically characterized the single-track molten pool behavior of walnut shell/co-polyester (Co-PES) composite powder across a wide parameter space. The model, which maintains a deviation of less than 10% between simulated and measured center temperatures, serves not only as a theoretical tool for optimizing selective laser sintering (SLS) manufacturing parameters but also as a transferable methodology applicable to other biomass-based composite systems. Looking forward, the integration of the validated model with in-situ monitoring and closed-loop control strategies holds considerable promise for enabling intelligent, defect-free additive manufacturing of sustainable biomass composites, contributing to the broader goal of advancing environmentally responsible manufacturing technologies.
ACKNOWLEDGMENTS
This work was supported by the Supported by Opening Project of the Key Laboratory of Advanced Manufacturing and Intelligent Technology(Ministry of Education), Harbin University of Science and Technology(KFKT202512), Guided Innovation Fund project of Northeast Petroleum University (2022YDL-06), National Cultivation Fund Project of Northeast Petroleum University (2024GPL-10), the Joint Scientific and Technological Innovation Project of Hainan Province (2021CXLH0001), Key R&D Program of Heilongjiang Province, China (JD2023SJ23), General Research Project of Higher Education Reform in Heilongjiang Province (SJGYY2024186), and the Scientific Research Start-up Fund Project of Northeast Petroleum University (2021KQ09 and 2019KQ67).
REFERENCES CITED
Amorim, F. L., Lohrengel, A., Neubert, V., Higa, C. F., and Czelusniak, T. (2014). “Selective laser sintering of Mo-CuNi composite to be used as EDM electrode,” Rapid Prototyping Journal 20(1), 59-68.
https://doi.org/10.1108/RPJ-04-2012-0035
Idriss, A. I. B., Li, J., Wang, Y., Guo, Y., and Elfaki, E. A. (2020). “Effects of various processing parameters on the mechanical properties of sisal fiber/PES composites produced via selective laser sintering,” BioResources 15(3), 5710-5724. https://doi.org/10.15376/biores.15.3.5710-5724
Jonkers, N., Dijk, W.J., Vonk, N. H., Dommelen, J. A. W., and Geers, M. G. D. (2022). “Anisotropic mechanical properties of selective laser sintered starch-based food,” Journal of Food Engineering 318, article 110890 https://doi.org/10.1016/j.jfoodeng.2021.110890
Kamboj, N., Ressler, A., and Hussainova, I. (2021). “Bioactive ceramic scaffolds for bone tissue engineering by powder bed selective laser processing: A review,” Materials 14(18), article 5338. https://doi.org/10.3390/ma14185338
Liu, J. H., Shi, Y. S., Liu, Z. L., Xu, Y., Chen, K. H., and Huang, S. H. (2007). “Manufacturing metal parts via indirect SLS of composite elemental powders,” Materials Science and Engineering: A 444(1-2), 146-152. https://doi.org/10.1016/j.msea.2006.08.070
Panwisawas, C., Qiu, C., Anderson, M. J., Sovani, Y., Turner, R. P., Attallah, M. M., Brooks, J. W., and Basoalto, H. C. (2017). “Mesoscale modelling of selective laser melting: Thermal fluid dynamics and microstructural evolution,” Computational Materials Science 126, 479-490. https://doi.org/10.1016/j.commatsci.2016.10.011
Salmoria, G. V., Klauss, P., Paggi, R. A., Kanis, L. A., and Lago, A. (2009). “Structure and mechanical properties of cellulose based scaffolds fabricated by selective laser sintering,” Polymer Testing 28(6), 648-652. https://doi.org/10.1016/j.polymertesting.2009.05.008
Yi, H., Qi, L., Luo, J., and Li, N. (2018). “Hole-defects in soluble core assisted aluminum droplet printing: Metallurgical mechanisms and elimination methods,” Applied Thermal Engineering 148, 1183-1193. https://doi.org/10.1016/j.applthermaleng.2018.12.013
Yi, H., Qi, L., Luo, J., Zhang, D., Li, H., and Hou, X. (2018). “Effect of the surface morphology of solidified droplet on remelting between neighboring aluminum droplets,” International Journal of Machine Tools and Manufacture 130, 1-11. https://doi.org/10.1016/j.ijmachtools.2018.03.006
Yu, Y. Q., Guo, Y. L., Jiang, T., Li, J., Jiang, K. Y., Zhang, H., and Zhuang, Y. (2018). “Study on the characteristics of walnut shell/co-PES/co-PA powder produced by selective laser sintering,” Materials 11(5), article 784. https://doi.org/10.3390/ma11050784
Yu, Y. Q., Jiang, M. Z., Wang, S. L., Guo, Y. L., Jiang, T., Zheng, Z. M., Huang, S. Q., Cui, T. Q., and Sha, K. (2021). “Dynamic evolution simulation of melt pool in selective laser sintering walnut shell/Co-PES composite,” Optics & Laser Technology 144, article 107425. https://doi.org/10.1016/j.optlastec.2021.107425
Zhang, H., Dengke, D., Shaopu, S., and Chen, A. (2019). “Experimental study of effect of post processing on fracture toughness and fatigue crack growth performance of selective laser melting Ti-6Al-4V,” Chinese Journal of Aeronautics 32(10), 2383-2393. https://doi.org/10.1016/j.cja.2018.12.007
Zhang, Y. H., Wang, F. M., Zhang, Y. F., Li, J., and Guo, Y. L. (2021). “Effect of Al powder on mechanical properties and microstructure of wood-plastic composites by selective laser sintering,” Materials Today Communications 27, article 102235 https://doi.org/10.1016/j.mtcomm.2021.102235
Zhao, D. J., Guo, Y. L., Song, W. L., and Jiang, K. Y. (2015). “Preparation and forming characteristics of bamboo flour/co-polyamide laser sintering composite,” Journal of Northeast Forestry University 43(6). 107-109, 115.
https://doi:10.13759/j.cnki.dlxb.2015.06.003
Article submitted: April 10, 2026; Peer review completed: May 3, 2026; Revised version received: May 26, 2026; Accepted: September 5, 2026; Published: October 12, 2026.
DOI: 10.15376/biores.21.4.11467-11482