NC State
BioResources
Soosairaj, J., Palanisamy Sathishkumar, T., Nagarajan, R., Krishnan, K., Yusof, N. A., and Mohammad, F. (2026). "Optimization of wear behavior in 3D-printed polylactic acid-based composites reinforced with carbon and wood particles," BioResources 21(4), 11622–11647.

Abstract

Optimization of Wear Behavior in 3D-printed Polylactic Acid-based Composites Reinforced with Carbon and Wood Particles

Wear characteristics were evaluated for 3D-printed polylactic acid (PLA) composites reinforced with wood particles and carbon fiber. The goal was enhanced robustness and wear resistance. Specimens were fabricated by fused deposition modelling and tested on a pin-on-disc tribometer in agreement with ASTM G99-23. Load, sliding speed, and sliding distance were considered as three primary factors with three-level Box–Behnken design. Analysis of variance (ANOVA) confirmed statistically significant regression models for both composites (F = 32.48, PLA-wood; F = 16.38, PLA-carbon fiber; p ≤ 0.003). Applied load was the dominant factor influencing wear rate, contributing 44.1% for PLA-carbon fiber and 44.9% for PLA-wood, followed by sliding velocity (12.6% and 21.0%, respectively) and sliding distance (5.60% and 9.35%, respectively). Wear rate increased with load (10 to 30 N) and sliding velocity (2.19 to 3.76 m/s) but stabilized at longer sliding distances (up to 2871 m) due to tribofilm creation. PLA/carbon fiber composites showed lower wear than PLA/wood particle composites, which was ascribed to higher hardness, improved load-bearing capacity, and development of a stable transfer layer. Scanning electron microscopy indicated severe fiber pull-out, voids, and delamination in PLA/wood specimens, whereas PLA/carbon fiber specimens established a protective tribofilm with minimal damage of carbon fiber.


Download PDF

Full Article

Optimization of Wear Behavior in 3D-printed Polylactic Acid-based Composites Reinforced with Carbon and Wood Particles

Jeyaraj Soosairaj,a,* Thottyeapalayam Palanisamy Sathishkumar,b Rajini Nagarajan,c,* Kumar Krishnan,d Nor Azah Yusof,e and Faruq Mohammad f

Wear characteristics were evaluated for 3D-printed polylactic acid (PLA) composites reinforced with wood particles and carbon fiber. The goal was enhanced robustness and wear resistance. Specimens were fabricated by fused deposition modelling and tested on a pin-on-disc tribometer in agreement with ASTM G99-23. Load, sliding speed, and sliding distance were considered as three primary factors with three-level Box–Behnken design. Analysis of variance (ANOVA) confirmed statistically significant regression models for both composites (F = 32.48, PLA-wood; F = 16.38, PLA-carbon fiber; p ≤ 0.003). Applied load was the dominant factor influencing wear rate, contributing 44.1% for PLA-carbon fiber and 44.9% for PLA-wood, followed by sliding velocity (12.6% and 21.0%, respectively) and sliding distance (5.60% and 9.35%, respectively). Wear rate increased with load (10 to 30 N) and sliding velocity (2.19 to 3.76 m/s) but stabilized at longer sliding distances (up to 2871 m) due to tribofilm creation. PLA/carbon fiber composites showed lower wear than PLA/wood particle composites, which was ascribed to higher hardness, improved load-bearing capacity, and development of a stable transfer layer. Scanning electron microscopy indicated severe fiber pull-out, voids, and delamination in PLA/wood specimens, whereas PLA/carbon fiber specimens established a protective tribofilm with minimal damage of carbon fiber.

DOI: 10.15376/biores.21.4.11622-11647

Keywords: PLA; Carbon fiber; Wood; Wear resistance; ANOVA; Process innovation

Contact information: a: School of Mechanical Engineering, SASTRA Deemed to be University, Thanjavur, Tamil Nadu, India; b: Materials Research Centre, Department of Mechanical Engineering, Kongu Engineering College, Erode, Tamil Nadu, India; c: Department of Mechanical Engineering, Kalasalingam Academy of Research and Education, Krishnankoil-626126, India; d: INTI International University, Persiaran Perdana BBN, 71800 Nilai, Negeri Sembilan, Malaysia; e: Department of Chemistry, Faculty of Science, Universiti Putra Malaysia, Serdang, Selangor, 43400 Malaysia; f: Department of Chemistry, College of Science, King Saud University, P.O. Box 2455, Riyadh, 11451 Kingdom of Saudi Arabia;

* Corresponding authors: [email protected]; [email protected]

Graphical Abstract

Optimization of Wear Behavior in 3D-printed Polylactic Acid-based Composites Reinforced with Carbon and Wood Particles

INTRODUCTION

The emerging demand for advanced wear-resistant materials is contributing to modernization across the automotive, aerospace, industrial construction, and wider engineering sectors. Polylactic acid (PLA) is a compostable, biodegradable, high-strength aliphatic polyester based thermoplastic extracted from renewable resources such as corn starch, cassava, and sugarcane wastes, and it is extensively utilized in biocompatible medical devices and industrial packaging systems (Nampoothiri et al. 2010; Joseph et al. 2023). Its prime advantages include ease of fabrication, biodegradability, and moderately low environmental impact in comparison to petroleum-based polymers, along with high stiffness, good flexibility, and aptness for fabrication via FDM 3D printing. 3D printing plays an essential role in sustainable manufacturing, empowering the fabrication of intricate parts and lightweight components, particularly in the aerospace, automotive segment, with reduced costs, greater processing speeds, and high precision fabrication.

Paulo Davim et al. (2020) reported that the evolution of new materials is a primary focus in progressing the structural viability of manufacturing processes. Research investigations in the arena of advanced mechanical engineering has progressively emphasized approaches to upgrade the tribological and comprehensive mechanical performance of extensively used thermoplastics such as PLA fabricated through Fused Deposition Modelling (FDM). Simultaneously, research works are extending into metal-based 3D printing, particularly the characterization and optimization of eco-degradable alloys. Accurate control of FDM printing parameters for these high-performance materials remains critical for restraining interfacial defects, controlling fatigue degradation, and certifying reliable material characteristics under challenging load-bearing conditions. Wang et al. (2024) studied present polymer processing techniques intended at enhancing the ease of printing, mechanical, and functional characteristics of 3D-printed PLA, while Hussain et al. (2024) investigated PLA characterization, engineering properties, biomedical applications, biodegradation. The work emphasized composite preparation and modeling and optimization as key research guidelines. In spite of its ease of process and eco-friendly nature, PLA suffers from intrinsic limitations in strength and endurance that limits its usage in challenging engineering applications; addressing these deficiencies is therefore important to intensifying its practical efficacy. To this end, composite materials such as PLA-carbon fiber and PLA-wood have been developed to enhance the mechanical and wear properties of PLA while preserving its sustainability.

A number of studies have suggested that combining additive manufacturing with composite reinforcement can improve wear performance. Jimenez and Bermudez (2011) investigated the fundamental mechanisms of dry sliding wear and friction in sliding contacts, together with their associated friction coefficients, identifying adhesion, stick-slip behavior, and ploughing as key frictional mechanisms, and describing wear in terms of erosive, adhesive, micro-abrasive, and corrosive processes. Their work also established the close relationship between friction and wear, positioning wear modelling as a valuable tool for predicting wear behavior under varying operating conditions and providing a strong foundation for understanding tribological performance in sliding contacts. More recent bibliometric analyses point to a substantial broadening of the field, with research shifting from traditional friction and wear management toward emerging subfields such as nanotribology, bio-tribology, and green tribology; from a functional engineering perspective, tribology captures the complex interactions among surface morphology, material degradation, and contact mechanics (Ismail et al. 2023; Davim et al. 2025).

For optimization of operational and experimental parameters governing 3D-printed polymers, researchers have focused on the progression from unreinforced matrices to multi-phase composite systems. The initial studies focused on optimizing fused filament fabrication (FFF) processing parameters such as infill density, layer thickness, and printing temperature to minimize surface roughness and wear loss in neat PLA. Building upon these reference line matrix optimizations, successive efforts have considered particulate fillers to improve dimensional stability and wear resistance; at this juncture, statistical tools including Response Surface Methodology (RSM) were employed to optimize filler loading alongside printing parameters (Ayyanar et al. 2026). Very recently, high-performance short-fiber reinforcements such as carbon fibers, have been combined into PLA to improve mechanical load bearing and thermal stability under dry sliding contact (Ning et al. (2015). A methodical relative optimization that simultaneously appraises the tribological investigations, transfer film formation, and thermal dissipation studies between low-cost wood particles and high-strength carbon fibers under identical multi-factor operational conditions remains not investigated.

Rachaiah et al. (2024) reported that incorporating graphene particles can improve the wear performance of PLA compounds, underscoring the potential of high-strength fiber reinforcements such as carbon fiber for improved functional performance. Louvis et al. (2011) found that selective laser melting, with appropriate process control, can significantly improve the mechanical and wear properties of aluminum-based products. Keshavamurthy et al. (2023) showed that 3D-printed composites reinforced with solid lubricants exhibit reduced friction and wear, improving their suitability for high-performance applications, and Kumar et al. (2022) compared 3D-printed AlSi10Mg components with conventionally stir-cast composites, reporting that 3D printing offers higher wear resistance owing to enhanced microstructural characteristics. Wood-particle-based composites represent an increasingly dynamic class of engineered wood materials that have followed a sustained trajectory of rapid development. Owing to their flexibility and favorable performance profile, these composites are gaining global traction as feasible, eco-friendly alternatives to conventional structural materials such as concrete, metals, and polymers, with recent work focusing on functionalized laminate structures, chemical and physical activation of natural fibers, bio-based matrices, and industrial manufacturing innovations in wood-composite engineering (Aguilera 2017).

Rajole et al. (2022) found that embedding alumina and silica fillers into polymer composites enhances mechanical toughness and wear resistance, while Mohamed et al. (2018) showed that 3D printing process parameters significantly influence wear behavior in PC-ABS components, underlining their importance in optimizing the wear resistance of PLA composites. Collectively, these studies indicate that PLA/carbon fiber composites combine the stiffness and strength of carbon fiber with the biodegradable, lightweight characteristics of PLA, making them well suited to high-mechanical, load-bearing applications, while PLA/wood-particle composites pair aesthetic appeal with improved toughness, making them attractive for engineering applications where both mechanical integrity and visual appearance are important. These findings highlight the need for further investigation of multifunctional PLA-based composites with tailored mechanical and sensing capabilities.

Response Surface Methodology (RSM) is a robust statistical technique for optimizing experimental parameters and the corresponding response properties, and the Box–Behnken Design (BBD) is among its most widely used approaches. Several studies have explored the application of such optimization techniques to the processing of PLA-based composites. Balasubramanian et al. (2025) optimized the mechanical behavior of 3D-printed PLA reinforced with Terminalia chebula nanoparticles, achieving a maximum tensile strength, while Mishra et al. (2025) optimized the fracture toughness of 3D-printed PLA/carbon fiber composites using a Taguchi–Grey Relational Analysis (GRA) approach to identify optimal material-extrusion parameters for improved mechanical performance. Patil et al. (2024) applied RSM to optimize the process parameters of 3D-printed PLA for enhanced tensile and flexural strength, and Calles et al. (2022) used a full factorial design of experiments to evaluate the tensile strength of 3D-printed PLA and carbon-fiber-reinforced PLA, identifying material type and perimeter settings as the most influential factors. Altan et al. (2018) examined the surface roughness of fused-deposition-modelled components as a function of layer thickness and nozzle temperature, concluding that surface roughness is strongly dependent on layer thickness, while Abeykoon et al. (2020) studied ABS and PLA printing parameters and found that synchronized printing speed and nozzle temperature are essential for proper melting and controlled solidification. Grasso et al. (2018) revealed that the strength and stiffness of 3D-printed PLA structure depend securely on infill direction and printing temperature, influenced by filament deformation closer to the glass transition section. Khan et al. (2013) prepared and investigated the mechanical properties of the MDF board reinforced with carbon fibre particles and revealed that stronger interfacial bonding was obtained between the carbon fibre and the matrix polymer. Addition of carbon fibres improved the mechanical strength and Internal Bonding (IB). Among the various preparations, composites containing 0.1 wt% of carbon fibers furnished the maximum enhancement in both physical and mechanical properties. Modern production increasingly leverages the complementary strengths of additive manufacturing (AM) and subtractive manufacturing (SM) to offset the limitations of each: additive processes such as 3D printing, fused deposition modelling, selective laser sintering, and electron beam melting offer exceptional geometric design freedom, customizability, and reduced material waste, whereas subtractive techniques provide precise tolerances and high surface integrity but incur significant material waste and tool wear when machining hard-to-process alloys, Davim et al. (2020).

In view of the growing demand for materials that are both sustainable and high-performing, enhancing the mechanical and wear properties of PLA through composite reinforcement and process optimization has become essential. Although previous studies have demonstrated improvements through various fillers and manufacturing parameters, comprehensive optimization of 3D-printed PLA/carbon fiber and PLA/wood composites remains limited. The present study therefore focuses on systematically investigating and optimizing key process parameters using response surface methodology to improve wear performance and tribological characteristics, thereby expanding the applicability of PLA-based composites in advanced engineering applications.

EXPERIMENTAL

Materials and Specimen Preparations

PLA/carbon fiber and PLA/wood composite filaments were selected as feedstock materials for the fabrication of the test specimens. These filaments were chosen to investigate the influence of fiber and natural filler reinforcement on the mechanical and structural characteristics of PLA-based composites. All the specimens were fabricated using the Bambu Lab A1 Combo 3D Printer, a high-precision, MEX-based additive manufacturing system equipped with an automatic material system (AMS) for multi-filament handling and consistent extrusion control. The printer is appropriate for processing composite filaments because it provides precise dimensional stability, effective temperature control, and a smooth surface finish.

The 3D printing parameters were carefully controlled for each carbon and wood filaments to achieve greater interlayer bonding and minimize defects. Chief parameters, such as nozzle temperature, bed temperature, printing speed, layer thickness, and infill density, were attuned based on the material structures and manufacturer references. This optimization authenticated the defect-free manufacture and mechanically reliable specimens for succeeding testing and characterization studies. Optimized printing parameters are maintained cautiously printing of the composite specimens under, keeping a bed temperature of 60 °C, a printing nozzle temperature of 220 °C, and a printing speed of 120 mm/s to ensure consistent layer deposition and dimensional stability.

The printing filament composition contained of approximately 20% carbon fiber and 80% PLA matrix base, for fabrication of the PLA/carbon fiber composite, a ratio chosen for balanced printability with improved mechanical reinforcement. The presence of carbon fiber observed notable enhancement in dimensional stability tensile strength, stiffness, and of the material compared to pure PLA. During fabrication, the filament exhibited minimal distortion, virtuous layer bonding, and unvarying extrusion, resulted with superior surface finish and reduced interior imperfections. The above-stated properties make PLA/carbon fiber composites well suited for structural and load-bearing applications that demand higher mechanical performance while maintaining the ease of processing typical of PLA.

Prepared PLA-Carbon fiber and PLA-wood specimens

Fig. 1. Prepared PLA-carbon fiber and PLA-wood specimens

Conversely, the PLA+Wood composite filament, made-up of 20% finely milled wood powder and 80% PLA, was prepared to replicate the natural texture and aesthetic appeal of wood while maintaining the printability and decomposability of PLA. This composite possessed smoother extrusion, steady flow of PLA, and reliable interlayer bonding while printing. Its wood-like appearance, lighter weight, and enhanced surface finish made it ideal for industrial products, CAD models, and artistic parts where both strength and aesthetic appeal are vital, even though its mechanical strength was only reasonable in comparison to PLA-carbon fiber alternative. The printed carbon fiber and wood particle specimens are shown in the Fig. 1.

EXPERIMENTAL SETUP

The wear test of the fabricated PLA-based composite specimens was carried out using a computerized Pin-on-Disc tribometer, a well-equipped device for evaluating the sliding wear behavior of testing materials under controlled laboratory conditions, in agreement with the ASTM G99 – 23 standard. The Pin on disc wear tester, as shown in Fig. 2, consists of a rotating EN31 alloy steel disc and a specimen pin mounted namely PLA–Carbon fiber and PLA–Wood. The EN31 disc, a high-carbon, high-chromium bearing steel, was chosen due to its excellent hardness, strength, and wear resistance, making it a suitable counter face material for polymer-based composites as per the ASTM standards. The disc had a hardness of 60 HRC, and a maximum wear track diameter of 120 mm, which assured minimal wear and highly durable of the counter surface during testing.

Pin-on-disc tribometer

Fig. 2. Pin-on-disc tribometer

The PLA pin specimens, each of 10 mm diameter and cylindrical shape, were brought into straight contact with the rotating EN31wear track disc under a given normal load condition. During testing, the pin retained stationary, a distinct circular wear track seemed on the disk surface as the disk rotated at a predetermined pace. This experimental arrangement made it feasible for sliding contact to be distributed consistently and allowed for wear characteristics to be determined consistently. The hardness of EN31 disc and surface quality assured that the mainstream of material loss occurred on the composite pins, permitting accurate estimation of the PLA-based composites’ wear rate.

The wear experiments were executed by carefully adjusting the applied load, sliding speed, and time period to evaluate the collective effect on the wear performance of the PLA/Wood and PLA/ Carbon fiber composites. In order to resemble actual operating conditions, these values were meticulously chosen within a prescribed interval. To understand the tribological behavior of the materials, the resulting wear rate and frictional properties were recorded and studied. This experimental setup offered a reliable technique to investigate material removal mechanisms, surface interactions, and the ideal combination of process parameters that reduced wear rate of PLA composites under experimentation.

Design of Experiments

In an experimental optimization approach having continuous parameters as inputs, a sequential optimization technique called Response Surface Methodology (RSM) can be employed. To determine the optimal operating conditions, tools such as Box-Behnken Design (BBD) and Central Composite Design (CCD) map 3D response surfaces can be chosen for optimization, reported by Astakhov (2012).

In this experimentation, prediction models were generated, and the influence of process factors was measured within predetermined frame work using the Box-Behnken Design, a subdivision of response surface methodology (RSM). The experiment response can be represented as a function of the distinct input process parameters when they are defined, as shown in Eq. 1.,

(1)

where j = 1, 2, ……., N signifies the N data point in the factorial experiment, yij = the level of the ith factor in the jth observation, and ej = residual quantity error of the jth observation. The function ψ is termed the response surface. The response variable (ψ) was statistically approached within the experimental sphere by means of polynomial equations expressed from the identified process variables. These polynomial models are widely employed in RSM because they can accurately represent the relationship between independent parameters and the connected output responses. One of the key advantage of using a polynomial response surface is that, even in scenarios when the behavior of the structure is complex, it is moderately easy and flexible to fix experimental data. Because it can excellently signify both the linear and interaction effects of the process variables, a quadratic polynomial function is commonly chosen among other model types. For example, the quadratic model typically has ten coefficients in a three-variable system, which is adequate to explain the response surface without being very difficult computationally. In an experimental system governed by three independent process variables, represented as y1, y2, and y3, the connection between the response and these input parameters can be efficiently denoted using a second-order (quadratic) polynomial model, as stated in Eq. 2:

(2)

In this equation, Z represents the predicted response value; b0 is the intercept or constant terms; b1, b2, and b3 correspond to the linear coefficients reflecting the individual effect of each variable, b11, b22, and b33 denote the quadratic coefficients accounting for curvature effects, and b12, b13, and b23 represent the interaction (cross-product) coefficients that describe the combined influence of two variables on the response. Such a quadratic model affords an inclusive depiction of both the main and interactive effects of the experimental parameters within the experimental design frame. It is particularly useful in RSM for optimizing process conditions, as it enables the prediction of response trajectories and the establishment of optimal parameter data set with minimum number of experiments.

The coefficients of the polynomial equations were assessed using a multiple regression model, and these coefficients were then employed to develop empirical equations for prediction of response value. Precise modelling of the experimental behavior within the experimental area is achieved by the regression coefficients, which significantly reflect the influence of each process parameter and their interaction combinations on the response output. The total number of experimental runs required for building a BBD is calculated by the following equation,

(3)

where k denotes the number of process variables or factors, and Co ​ represents the number of central points comprised to ensure model accuracy estimate and the experimental error.

In the current study, with three experimental factors (k=3) each set at three levels (−1, 0, +1), the BBD necessitates a total of 15 experimental runs. This design proficiently allocates the experimental points covering the design frame without considering extreme corner points, in that way minimizing the number of experimental runs while sustaining the ability to fit a full quadratic model for the design. In conclusion, the BBD constitutes a cost-effective and statistically robust design for developing response surface models and optimizing process parameters for reliable and consistent experimental design. Table 1 indicates that load (L), sliding speed (V), and sliding distance (S) were the wear testing parameters considered in the present research. These features were found to be the parameters with the greatest significance impacting the wear rate of the composite specimens during the pin-on-disc wear test.

Table 1. Input Parameters Taken for Experimentation

Input Parameters Taken for Experimentation

The sliding speed and sliding distance are inherently dependent on the turning speed (N) of the disc and the test duration (t), and their relationships are expressed mathematically in Eqs. 4 and 5. To confirm regularity and steadiness in the experimental design, equal intervals were consequently allocated for the rotating speed and trail run time values agreeing to the selected parameter levels.

The sliding distance (S) denotes the overall linear distance travelled by the specimen surface against the rotating disc during the test run, was computed using the following Eq. 4:

Sliding distance, in m = Sliding speed (m/s) × time (s)    (4)

The sliding speed (V) indicates the relative velocity between the test specimen and the steel disc, was determined based on the rotational speed of the steel disc and the diameter of the wear track using Eq. 5,

Sliding Speed (m/s) = Π × D × N/60   (5)

where D is the diameter of the wear track (m) and N is the rotation speed (rpm).

These equations designate the direct connection between the rotary motion of the wear disc and the linear motion accomplished at the contact surface of specimen. By maintaining constant intervals for test period and rotation speed, a consistent and organized variation of sliding speed and sliding distance was observed across all experimental trial runs. This design approach guaranteed reliable data procurement and assisted accurate estimation of the combined impact of load, speed, and distance on the wear characteristics of the composite specimens.

In this investigation, the wear rate was acknowledged as the principal response variable. It was assessed based on the mass loss approach, where the mass of each test specimen was determined both before and after the wear test trail using a high-precision digital weighing balance. The difference in mass between the pre-test and post-test measurements was considered to calculate the wear rate, thereby computing the material loss under standard test conditions. The experimental density of the 3D-printed composite test specimens was measured using the Archimedes immersion method in distilled water according to ASTM D792. Measurements were determined at 23 °C using a high-precision digital analytical balance (SHIMADZU analytical balance, Japan – Type AUX220, Min. 0.1mg,). The measured composite densities were:

PLA/Wood composite density (ρwood): 1.205 ± 0.012 g/cm3 (1.205×10−3 g/mm3)

PLA/Carbon fiber composite density (ρCF): 1.298 ± 0.015 g/cm3 (1.298×10−3 g/mm3)

The mass loss was determined by weighing each specimen before and after every experimental run using a precision balance, and the obtained values were then used to estimate the wear rate according to Eqs. 6 and 7:

Mass loss (g) = mass before exp. (g) – mass after exp. (g)         (6)

Wear rate = mass loss (g)/ [Density (g/mm3) × Sliding distance (m)]        (7)

All the experimental trials were conducted following identical procedures to ensure repeatability and minimize systematic errors.

RESULTS AND DISCUSSION

Tabulated Results

The obtained experimental results, including the corresponding combinations of process parameters and the measured wear rate values, are compiled and presented in Table 2 for subsequent statistical analysis and model validation.

In the experimental arrangement, the Box–Behnken Design (BBD) statistical response surface was specifically built to model and optimize specific wear rate (W) as the prime response variable. In the same way, friction force was documented continuously using a calibrated piezo-electric load cell coupled to the Pin-on-Disc data acquisition software throughout every 15-run experimental trial. The PLA / Wood Composite exhibited an average steady-state value of COF ranging from 0.32 to 0.44 (mean COF ≈ 0.38) and for PLA / carbon fiber ranging from 0.22 to 0.30 (mean COF ≈ 0.26).

Multiple regression analysis was developed to determine the coefficients of the quadratic polynomial presented in Eq. 2, with calculations performed using Minitab 16 statistical software.

Table 2. Experimental Data of PLA/Wood and PLA/Carbon Fiber Based on BBD

Experimental Data of PLA/Wood and PLA/Carbon Fiber Based on BBD

The resulting predictive model for wear (W) is presented below. Wear for 3D-printed PLA-Wood is given as:

Wear = 2.367 + 0.63L + 0.431V – 0.288S + 0.191L2 + 0.241V2+ 0.057S2 + 0.432LV – 0.367LS + 0.062VS        (8)

whereas the wear for 3D-printed PLA-Carbon Fiber is given as:

Wear = 1.595 + 0.393L + 0.211V – 0.14S + 0.107L2 + 0.196V2 + 0.008S2 + 0.297LV – 0.29LS + 0.161VS           (9)

The wear test results reveal that the wear rate of PLA/wood composites was higher than that of PLA/carbon fiber composites. The results indicate that the wear resistance of PLA is improved through reinforcement with both wood and carbon fibers, with carbon fiber reinforcement yielding better performance.

Direct Effect of Process Parameters on Wear Rate

The developed statistical model was used to predict the wear rate using selected values of the process parameters. The influence of these parameters on the wear behavior of 3D-printed PLA/wood and PLA/carbon fiber composites was analyzed using the empirical model.

Figure 3 (a) illustrates the direct effect of applied load on the wear rate of 3D-printed PLA/wood and PLA/carbon fiber composites at a constant sliding velocity of 3.76 m/s and a sliding distance of 2871 m. For both materials, the wear rate increased monotonically with increasing load, indicating load-dependent wear behavior. The PLA/wood composite steadily displayed a higher wear rate than the PLA/carbon fiber composite across all load conditions. At lower loads conditions (10 N), the wear of PLA/wood was ruled principally by minor adhesive wear. However, as the load increased, matrix softening, fiber pull-out, and fragmentation of wood particles occurred, generating loose debris that acted as third-body abrasive particles, thereby accelerating material removal and resulting in a sharp increase in wear rate. Conversely, the PLA/carbon fiber composite exhibited somewhat lower wear rates, increasing progressively with load. The dominant wear mechanism in PLA/carbon fiber was mild abrasive wear accompanied by the formation of a stable transfer layer on the counterface. The presence of hard carbon fibers enhanced load-bearing capacity, limited plastic deformation of the PLA matrix, and suppressed severe adhesive wear even at higher loads, leading to improved wear resistance.

Figure 3 (b) illustrates the direct effect of sliding velocity on the wear rate of 3D-printed PLA/wood and PLA/carbon fiber composites at a constant applied load of 30 N and a sliding distance of 2871 m. For both composites, the wear rate increased with increasing sliding velocity, indicating velocity-dependent wear behavior. The PLA/wood composite exhibited a consistently higher wear rate across the entire range of sliding velocities compared to the PLA/carbon fiber composite. At lower sliding velocities (2.19 m/s), the wear of PLA/wood was relatively mild and dominated by adhesive wear. However, with increasing sliding velocity, frictional heating intensified, leading to softening of the PLA matrix and increased fiber pull-out. The generated debris promoted three-body abrasive wear, resulting in a sharp rise in wear rate at higher velocities. In contrast, the PLA/carbon fiber composite showed a gradual increase in wear rate with sliding velocity. The dominant wear mechanism was mild abrasive wear accompanied by the formation of a stable transfer film on the counterface. This incident was certified by Basboga (2023). The presence of carbon fibers enhances thermal stability, improves load sharing, and reduces matrix softening, thereby suppressing severe adhesive wear even at higher sliding velocities.

Figure 3 (c) shows the direct effect of sliding distance on the wear rate of 3D-printed PLA/wood and PLA/carbon fiber composites at a constant applied load of 30 N and a sliding velocity of 3.76 m/s. For both composites, the wear rate decreased with increasing sliding distance, indicating the occurrence of a running-in wear regime followed by a more stable wear behavior. It was observed that there was a decrease in distinct volumetric wear rate (W) with increasing sliding distance (S) for the PLA/Wood particle composite. This behavior is ascribed to the changeover from initial run-in wear to a stabilized steady-state sliding pattern developed by tribo-debris accumulation. As is apparent in Fig. 3c, increasing the sliding distance resulted in a continuing reduction in the specific wear rate of PLA/wood particle composites. This tendency indicates a shift from severe transient run-in wear conquered by high severity shear to a steady-state mechanism designated by the formation of an accumulated organic tribo-film, as reported by Almeshaal et al (2026). Sheared wood debris combines under repetitive sliding contact, filling surface micro-grooves and creating a protective transfer layer that allocates normal stresses and condenses consequent volumetric loss over protracted distances.

Direct effect of process parameters on wear rate

Fig. 3. Direct effect of process parameters on wear rate

Interaction Effect of Process Parameters on Wear Rate

The interaction effect examines how the impact of one process parameter on the response varies with changes in a second parameter, while all other parameters are maintained at their mid-levels. This analysis offers insight into the wear behavior of the fabricated specimens when two parameters are evaluated simultaneously. The interaction effects of process parameters that significantly influence the wear rate were analyzed, evaluated, and plotted using statistical software (Minitab 16), as shown in Fig. 4 for PLA–wood composites and Fig. 5 for PLA–carbon fiber composites.

Figure 4 (a) shows the interaction effect of load and sliding velocity on the wear rate of 3D-printed PLA–wood composites. At lower loads (≈10 to 20 N) and moderate sliding speeds, the wear rate remained small, representing steady sliding conditions with negligible material removal. As the load rises, the wear rate increased progressively, and this effect became more distinct at higher sliding speed conditions. The combined effect of high load and high sliding velocity results in amplified contact stress and frictional heating, which develops the softening of PLA matrix and undermines the bonding between the polymer matrix and the wood particles. Therefore, severe adhesive and abrasive wear mechanisms control, leading to higher wear rates.

Figure 4 (b) shows the interaction effect of applied load and sliding distance on the wear rate of 3D-printed PLA–wood composites at a constant sliding velocity. At lower load conditions (≈10 to 20 N), the wear rate remains comparatively small across the entire level of sliding distances, representing minor and stable wear behavior. When applied load increased, a noticeable increase in wear rate was observed, and this increase became more significant with increasing sliding distance. At higher load conditions associated with higher sliding distances, the cumulative effect of repetitive contact and constant friction led to softening of matrix and pull-out of wood particles from the PLA matrix. This intensified material removal through leading abrasive and adhesive wear mechanisms.

Figure 4 (c) illustrates the interaction effect of sliding velocity and sliding distance on the wear characteristics of 3D-printed PLA–wood composites at a constant load condition of 30 N. The wear rate was minimal at lower sliding velocities and lesser sliding distances, signifying minimal wear and consistent tribological features. The wear rate rose progressively due to increases in sliding velocity, and this consequence became more noticeable with rising sliding distance. The combined effect of higher velocity and longer sliding distance yields amplified frictional heat zone and lengthy contact, which led to softer PLA matrix and greater debonding of the wood particles in the matrix. Elevated wear rates were triggered by the superiority of severe adhesive and abrasive wear progression.

Interaction effect of process parameters on wear rate (PLA/Wood)

Fig. 4. Interaction effect of process parameters on wear rate (PLA/Wood)

Figure 5(a) shows the interaction effect of load and sliding velocity on the wear rate of 3D-printed PLA–carbon fiber composites at a constant sliding distance. At lower load conditions (≈10 to 20 N) and modest sliding velocities, the wear rate was minimized, representing productive load-bearing by the presence of carbon fiber reinforcement and constant sliding conditions. As the applied load increased, the wear rate grew progressively, and this upsurge became more noticeable at higher sliding velocities. The combination effect of high load and high sliding velocity facilitates to increased contact stress and frictional heating, which can induce softening of PLA matrix and fiber–matrix interphase degradation. This promotes micro-cutting, fiber debonding, and pull-out, resulting in higher wear rates.

Figure 5(b) indicates the interaction effect of applied load and sliding distance on the wear rate of PLA–carbon fiber composites at a constant sliding speed of 3.76 m/s. At lower loads conditions (≈10 to 20 N), the wear rate was minimal over the entire level of sliding distances, representing improved reinforcement by carbon fibers and constant wear behavior. When applied load surged, the wear rate increased gradually, and this result became more noticeable with increasing sliding distance. The combination of higher load and longer sliding distance combinations resulted in high contact stress and aggregate frictional damage, promoting softening of PLA matrix and fiber–matrix interfacial deformation. Subsequently alternatives, such as fiber debonding, micro-ploughing, and fiber delamination, became foremost, triggering severe wear rates.

Interaction effect of process parameters on wear rate (PLA/carbon fiber)

Fig. 5. Interaction effect of process parameters on wear rate (PLA/carbon fiber)

The interaction effects between sliding velocity and sliding distance on the wear rate of PLA – carbon fiber composites under a constant load of 30 N are shown in Fig. 5(c). The wear rate remained low at lower sliding velocities and shorter sliding lengths, signifying the carbon fiber reinforcement’s efficient load-bearing capacity and defensive function. The wear rate progressively increased as the sliding velocity rose, and this consequence amplified as the sliding distance increased. Higher sliding velocity and longer sliding distance coordinated together to increase frictional heating and collective surface damage, which worsened the fiber–matrix structure and softened the matrix. Higher wear rates were significant for wear mechanisms such as fiber debonding, micro-cutting, and fiber pull-out behaviors.

ANOVA

ANOVA is a statistical tool used to investigate the influence of experimental factors on an outcome response variable by inspecting the mean sum of squares attained from experimental data. The data are typically obtained via well-framed robust experimental design. By assessing the inconsistency caused from controllable and uncontrollable experimental factors, ANOVA makes it possible to recognize which factors have a significant influence on the outcome response. The significance is computed using an F-test, which correlates the mean sum of squares of each parameter with the experimentation error at a selected confidence level.

Table 6 represents results of the analysis of variance (ANOVA) for the wear rate of the PLA–wood composite, appraising the impact of applied load (L), sliding velocity (V), and sliding distance (S), associated with their interaction and quadratic effects. The developed regression equation was statistically substantial, as validated by a higher F-value of 32.48 and a low p-value (p = 0.001), assuring that the designated process parameters efficiently clarify the difference in wear rate.

Table 6. ANOVA for Wear Rate in PLA/Wood Composite

ANOVA for Wear Rate in PLA/Wood Composite

Among the main effects, applied load (L) had the most important influence on wear rate, indicating the highest F-value (133.57) and the higher percentage of contribution (44.94%). This authenticates that increased normal load pointedly accelerated the material removal rate in the PLA–wood composite due to higher fiber delamination and contact stress. Sliding velocity (V) was identified as the second most influential factor contributing to the total variance. It showed a statistically significant effect on the wear rate, as designated by an F-value of 62.48 (F₁,₅) and a p-value of 0.001.Sliding distance (S) also showed an important effect on wear rate, with an F-value of 27.77 and 9.35 % of contribution, expressing progressive surface distortion with increased sliding period. The combination effects of L×V and L×S were statistically significant (p < 0.05), suggesting that the combined influence of load with sliding velocity or sliding distance played an active role in managing wear characteristics. Similarly, the interaction of V×S displayed a lower F-value (0.67) and a higher p-value (p = 0.451), indicating that this combination has an insignificant effect on wear rate. Quadratic relationships designate mixed significance. The V² attribute was statistically significant (p = 0.032), indicating a nonlinear effect of sliding velocity on wear rate. The quadratic term for applied load (L2) confirmed the statistical significance (F1,5 = 4.45, p = 0.089), while the quadratic term for sliding distance (S2) was not statistically significant (F1,5 = 0.50, p = 0.511), representing that sliding distance essentially influences wear rate through a linear relationship.

Table 7. ANOVA for Wear Rate in PLA/Carbon Fiber Composite

ANOVA for Wear Rate in PLA/Carbon Fiber Composite

Table 7 represents the ANOVA results for the wear rate of the PLA–carbon fiber composite, exploring the effects of applied load (L), sliding velocity (V), and sliding distance (S), in addition with their interaction and quadratic relations. The documented regression model was statistically significant, as indicated by an F-value of 16.4 and a p-value of 0.003, recognizing the adaptability of the model in connecting the wear behavior of the composite. Among the principal process parameters, applied load (L) exerted the most influencing factor on wear rate of PLA–carbon fiber, accounting for 44.06% to the total variation and achieving a high F-value of 67.17 with a statistically significant p-value (p < 0.001). This supports the important role of normal load in handling contact stresses and material removal rate through dry sliding. Sliding velocity (V) was the second most important factor, with a contribution of 12.62 % and an F-value of 19.24. This suggests that shear had significant effects and frictional heating harmed wear behavior. Sliding distance (S) also showed a statistically significant effect (p = 0.033), but a relatively lower contribution of 5.60%. The interaction effects L×V and L×S were statistically significant (p < 0.01), which indicates that the combined effect of load with sliding velocity or sliding distance contributed in a significant way to the wear rate. The V×S interaction was not significant (p = 0.064), indicating a weaker combined effect of these parameters. Corresponding to quadratic terms, the V² variable was statistically significant (p = 0.039), indicating a nonlinear relation between sliding velocity and wear rate. Further, L² (p = 0.244) and S² (p = 0.982) were not statistically significant, indicating mostly linear effects of load and sliding distance within the calculated range. The low residual error (sum of squares = 0.092) indicates strong agreement between the experimental and predicted wear rates.

For the PLA/Wood composite, the coefficient of determination (R2) was 0.9832 (98.32%), with an adjusted R2 (R2Adj) of 0.9529 (95.29%) and a predicted R2 (R2Pred) of 0.9145 (91.45%). Similarly, the PLA/Carbon Fiber composite model demonstrates strong statistical adequacy, yielding an R2 of 0.9672 (96.72%), an R2Adj of 0.9082 (90.82%), and an R2Pred of 0.8520 (85.20%). Both models met the benchmark requirement for a high-fitting regression model (R2 > 0.90). Additionally, the complete differences between R2Adj and R2Pred were 0.0384 for PLA/Wood and 0.0562 for PLA/Carbon Fiber; both were well below the suggested threshold limit of 0.20, assuring that neither model is over-fitted and both possess better reliability for prediction of wear rates within the experimental design frame.

Microstructure Examination

Figure 6 (a and b) shows the SEM micrographs of the surface of the PLA/wood composite prior to the wear test, captured at different magnifications. The surface morphology reveals the inherent structural appearances of the composite prepared from the FDM 3D printing process and the reinforcement of wood particles embedded in the PLA matrix. The micrograph evidently shows the presence of wood particles deposition in the PLA matrix, which is consistent with the effective reinforcement and fiber retention during filament extrusion and printing. The printed wood layer appeared moderately exposed at the surface, signifying non-uniform wood particle distribution and slight interfacial attachment between the PLA matrix and wood particles. Few micro voids and pores were detected on the surface, which can be ascribed to partial fusion between successive printed layers and moisture-induced degradation of wood particles during printing. These voids are distinctive in bio-filled PLA composites processed through additive manufacturing and may serve as stress concentration locations during mechanical or tribological loading. Also, particle pull-out topographies are evident, specifying weak interfacial bond between the wood particles and the PLA matrix. This weak adhesion can be connected with the hydrophilic character of wood particles and the hydrophobic PLA matrix, directing to poor stress transition at the interface.

SEM image of PLA/wood composite before wear test (a) 100 X and (b) 500 X