NC State
BioResources
Giagli, K., Vavrčík, H., Gryc, V., Tsalagkas, D., Brabec, M., Krajnc, L., Foltýnová, L., and Horáček, P. (2026). "Site-specific comparative density- and core-based assessment of mechanical properties in sessile and English oak from two Czech forest sites," BioResources 21(4), 12139–12168.

Abstract

Predicting oak wood quality is important for timber grading, forest management, and designing efficient wood-assessment workflows. This study compared destructive, semi-destructive, and dendrochronological approaches for evaluating wood quality in two contrasting stands in the Czech Republic: The SM stand is a sessile oak (Quercus petraea) upland forest and the JA stand is an English oak (Quercus robur) floodplain forest. The objective was to assess how effectively different measurement approaches capture variation in density and mechanical performance under realistic field conditions. Each species was sampled in a single representative stand; therefore, the study compares two stand-species combinations rather than isolating species effects from stand conditions. Sessile oak showed higher mean standard-specimen density (713 kg/m³ vs. 655 kg/m³), modulus of elasticity (9180 MPa vs. 8030 MPa), and modulus of rupture (93.6 MPa vs. 85.7 MPa) than English oak. Density was the strongest predictor of bending properties in both stand-species combinations, while latewood proportion improved interpretation of mechanical variation, especially when considered together with density. Compressive strength yielded the most consistent screening results, whereas Fractometer-derived outputs were more variable. The findings support density-based screening as the most robust practical approach, while also showing that compression-related relationships and dendrochronological indicators are more context-dependent.


Download PDF

Full Article

Site-specific Comparative Density- and Core-Based Assessment of Mechanical Properties in Sessile and English Oak from Two Czech Forest Sites

Kyriaki Giagli ,a,* Hanuš Vavrčík ,a Vladimír Gryc ,a Dimitrios Tsalagkas ,a Martin Brabec ,a Luka Krajnc ,c Lenka Foltýnová ,b and Petr Horáček , a,b

Predicting oak wood quality is important for timber grading, forest management, and designing efficient wood-assessment workflows. This study compared destructive, semi-destructive, and dendrochronological approaches for evaluating wood quality in two contrasting stands in the Czech Republic: The SM stand is a sessile oak (Quercus petraea) upland forest and the JA stand is an English oak (Quercus robur) floodplain forest. The objective was to assess how effectively different measurement approaches capture variation in density and mechanical performance under realistic field conditions. Each species was sampled in a single representative stand; therefore, the study compares two stand-species combinations rather than isolating species effects from stand conditions. Sessile oak showed higher mean standard-specimen density (713 kg/m³ vs. 655 kg/m³), modulus of elasticity (9180 MPa vs. 8030 MPa), and modulus of rupture (93.6 MPa vs. 85.7 MPa) than English oak. Density was the strongest predictor of bending properties in both stand-species combinations, while latewood proportion improved interpretation of mechanical variation, especially when considered together with density. Compressive strength yielded the most consistent screening results, whereas Fractometer-derived outputs were more variable. The findings support density-based screening as the most robust practical approach, while also showing that compression-related relationships and dendrochronological indicators are more context-dependent.

DOI: 10.15376/biores.21.4.12139-12168

Keywords: Quercus petraea; Quercus robur; Fractometer; Wood density; Modulus of rupture; Modulus of elasticity

Contact information: a: Mendel University in Brno, Faculty of Forestry and Wood Technology, Department of Wood Science and Technology, Zemĕdĕlská 3, 61300 Brno, Czech Republic; b: Global Change Research Institute of the Czech Academy of Sciences, Bělidla 986/4a, 60300 Brno, Czech Republic; c: Slovenian Forestry Institute, Večna pot 2, 1000 Ljubljana, Slovenia; *Corresponding author: [email protected]

INTRODUCTION

Sessile oak (Quercus petraea (Matt.) Liebl.) and English oak (Quercus robur L.) are key hardwood species in Central Europe, and their ecological differences associated with stand conditions, influence wood anatomy, density, and mechanical properties, require species-specific assessment methods (Cienciala et al. 2008; Vavrčík and Gryc 2012; Dobrovolný 2014; Eaton et al. 2016; Dobrovolný et al. 2017; Mölder et al. 2019; Wang 2021; Arenas-Navarro et al. 2021; Bölöni et al. 2021; Provost et al. 2022). Assessing wood quality at forest sites is vital for sustainable management and requires efficient, reliable, and practical methods suited to temperate forests. Systematic assessment combines visual, non-destructive, and destructive techniques to maximize information while conserving resources, and robust protocols must account for site-specific factors, species traits, and end-use needs to support forest management and timber use (Cienciala et al. 2008; May et al. 2017; Wang 2021; Ding et al. 2021). Reliable and timely quality assessment also depends on controlling biological variability, measurement error, and bias through calibration, training, and inter-laboratory comparisons, thereby supporting resource efficiency, and product reliability (Cienciala et al. 2008; Dobrovolný et al. 2017; Triplat and Krajnc 2017; Mölder et al. 2019; Březina et al. 2020; Gendvilas et al. 2024; Jönsson et al. 2025).

Previous studies have examined individual components of oak wood-quality assessment, including standard mechanical testing, increment-core analysis, and semi-destructive approaches, but the combined application of these methods within one design remains insufficiently documented, particularly where core-based indicators are directly cross-checked against standard mechanical testing outcomes (Vavrčík and Gryc 2012; Diaz-Maroto and Tahir 2018, 2019; Gendvilas et al. 2024). This study addresses this gap by comparing standard-specimen and increment-core measurements, dendrochronological traits, and Fractometer outputs within a single unified sampling protocol applied to two contrasting oak stand types in the Czech Republic (Dobrovolný 2014; Dobrovolný et al. 2017; Mölder et al. 2019; Špulák et al. 2024). The novelty is in comparing standard specimens, increment cores, and Fractometer outputs across upland sessile oak and floodplain English oak stands under one protocol, allowing direct assessment of how core-based and semi-destructive measurements reflect mechanical properties, without isolating patterns related solely to stand conditions.

Sessile oak typically occupies upland habitats with moderate water availability, whereas English oak is characteristic of lowland and floodplain forests with higher soil moisture; these contrasting ecological niches describe their growth conditions and are reflected in wood formation (Viewegh et al. 2003; Cienciala et al. 2008; Dobrovolný 2014; Mölder et al. 2019). Sessile oak is adapted to upland, well-drained sites with stronger support tissues and better drought tolerance (Vavrčík and Gryc 2012; Eaton et al. 2016; Löf et al. 2016; May et al. 2017; Diaz-Maroto and Tahir 2018; Giagli et al. 2018; Mölder et al. 2019; Wang 2021). English oak is associated with mesic to moist lowland habitats, including floodplains and river valleys. It can tolerate periodic waterlogging; however, its radial growth remains dependent on water availability and may be constrained by drought, especially where groundwater supply is limited (Heklau et al. 2019; Bose et al. 2021; Nosenko et al. 2025).

The contrasting sites occupied by sessile and English oak can modify cambial growth, vessel structure, tree-ring width, and the proportion of latewood, thereby influencing wood density and mechanical performance. Sessile oak growing on relatively well-drained upland sites often forms denser wood and may show higher stiffness and bending strength, whereas English oak from mesic or floodplain environments may show faster radial growth and lower density; however, these patterns are contingent upon local hydrology, provenance, tree age, and silvicultural history, and can be evaluated through systematic site-based methodologies across various environments (Vavrčík and Gryc 2012; Olarescu et al. 2016; Sejdiu et al. 2020; Hietz et al. 2022; Gryc et al. 2025).

Comparing oak species has revealed key differences in failure mechanisms and load distribution that affect timber performance in structural uses (Diaz-Maroto and Tahir 2019). Methodological challenges in oak wood quality assessment involve integrating multiple testing approaches to balance comprehensive characterization with efficiency in forest and processing environments. Species differences in compression strength are related to cell wall thickness, cell density, and the proportion of latewood, with English oak generally showing lower mechanical strength (Hirofumi et al. 2007; Diaz-Maroto and Tahir 2018, 2019). Destructive testing provides precise data but requires substantial material and time, while non-destructive and semi-destructive techniques such as acoustic velocity measurement, resistograph testing, and visual grading are better suited to initial screening (Mäkelä et al. 2010; Vavrčík and Gryc 2012; Merela and Čufar 2013; Llana et al. 2020). Combining methods within hierarchical protocols can improve efficiency and help identify the most suitable approach for each application (Hirofumi et al. 2007; Triplat and Krajnc 2017; Diaz-Maroto and Tahir 2018, 2019), while standardising mechanical testing equipment ensures reproducible, comparable results in research and industry (Merela and Čufar 2013; Bucur 2023).

Integrated testing with Zwick Z050, Tinius Olsen 10ST, and Fractometer II methods enables evaluation across scales from laboratory to field, with density, latewood, and compression-related traits influencing strength (Hirofumi et al. 2007; Diaz-Maroto and Tahir 2018, 2019; Zhang et al. 2024). The Zwick Z050/TH 3A machine standardises bending strength and elasticity measurements. The Tinius Olsen 10ST supports compression and strength tests on smaller specimens, providing standard conditions for assessing species- and site-specific differences. Multiple platforms enable comprehensive property assessments aligned with standards and specimen types. Compression testing focuses on load resistance, measured both parallel and perpendicular to the grain, and is crucial for structural applications involving oak timber under compression. Fractometer II enables semi-destructive bending-shear strength assessment from a forest management perspective, using 5-mm diameter core samples, suitable for on-site forest quality evaluation and ensuring statistical validity. Fractometer II assessment of bending-shear strength is an innovative approach that uses minimal material to reliably evaluate mechanical properties. This semi-destructive methodology supports field assessments of shear resistance, offering practical advantages for forest quality evaluations while maintaining reliability (Diaz-Maroto and Tahir 2019).

This study assessed the efficacy of diverse measurement methodologies in accurately capturing variations in density and mechanical performance under authentic field conditions. By sampling each species within a single representative stand, the potential confounding of species identity with stand conditions was acknowledged. Consequently, the study compared two stand–species combinations rather than isolating effects specific to individual species or stand condition patterns (Viewegh et al. 2003; Cienciala et al. 2008; Dobrovolný 2014; Dobrovolný et al. 2017; Mölder et al. 2019; Špulák et al. 2024). The primary objective of this research was to compare destructive, semi-destructive, and dendrochronological predictors of oak wood quality by assessing standard-specimen density (Zwick Z050), core-based density (Tinius Olsen 10ST and Fractometer II), tree-ring width, and latewood proportion in two contrasting stands—namely, an upland sessile oak stand and a floodplain English oak stand—selected to represent the typical ecological niches of these species within Czech forests. Additionally, the study examined the relationship between density and growth traits and their influence on bending and compression properties, thereby appraising the relative utility of destructive, semi-destructive, and dendrochronological methods for predicting oak wood quality across two distinct stand-species combinations.

EXPERIMENTAL

Stand Characteristics

Sessile oak (Quercus petraea (Matt.) Liebl.) was sampled in the Soběšice-Mokrohorská stand (SM; sessile oak upland stand). English oak (Quercus robur L.) was sampled in the Janohrad stand (JA; English oak floodplain stand). The SM stand (385 m a.s.l.) is characterized by well-drained soils and moderate water availability, whereas the JA stand (159 m a.s.l.) has moisture-rich, periodically inundated alluvial soils typical of lowland forests (Dobrovolný 2014; Dobrovolný et al. 2017; Mölder et al. 2019). These stand conditions reflect the ecological differentiation of the two species in Czech forests and provide the contrasting environmental background for the comparisons (Viewegh et al. 2003; Cienciala et al. 2008; Dobrovolný 2014; Mölder et al. 2019). Mean annual air temperature (Tav; calculated from annual means) and annual precipitation (PRCP; calculated from annual sums) were summarized for 1960 to 2025 using data from the Czech Hydrometeorological Institute open-data portal (opendata.chmi.cz). For the SM stand, Tav was 9.5 ± 1.1 °C and PRCP was 505.3 ± 82.6 mm; for the JA stand, Tav was 9.6 ± 0.9 °C and PRCP was 490.0 ± 93.6 mm (CHMI Open Data 2026). These values describe the climatic background of the two sampled stands and were not used to test ecological effects independently.

Table 1 shows all variables, units, and abbreviations for each test.

Table 1. Nomenclature of Variables, Units, and Abbreviations Used for Both Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand), across all Sample Types Included in the Study: C5 Dendrochronological and Fractometer Cores, C10 Compression Cores, and STS Bending Specimens

Nomenclature of Variables, Units, and Abbreviations Used for Both Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand)

Felled trees

In this work, six trees per stand (12 trees in total) were felled and sampled at two stem positions: breast height (1.3 m above ground, L) and the crown base (H). The average tree diameter and height for SM stand trees were 38.3 cm and 20.3 m; for JA stand trees, 48.5 cm and 29.43 m. Six trees per stand were felled, and twelve standing trees per stand were sampled with increment borers. The felled trees provided logs and discs for bending and dendrochronological analyses, whereas the cored trees provided C5 and C10 increment cores for dendrochronology, Fractometer testing, compression testing, and density determination. All logs and discs were labeled and stored to minimize moisture loss before laboratory analysis. The complete sampling and specimen-preparation workflow is shown in Fig. 1 and summarized in Table 2.

Table 2. Sampling Design for the Two Sampled Stands: SM; Sessile Oak Upland Stand (Quercus petraea), JA; English Oak Floodplain Stand (Quercus robur)

Sampling Design for the Two Sampled Stands: SM; Sessile Oak Upland Stand (Quercus petraea), JA; English Oak Floodplain Stand (Quercus robur)

Cored trees

Twelve standing trees per stand (24 trees in total) were sampled non-destructively with a Pressler increment borer. C10 cores were subdivided into 1-cm sections for compression testing and density determination, whereas C5 cores were marked at five-tree-ring intervals for Fractometer II testing and density determination (Fig. 1F, G).

All cores were stored in sealed tubes or straws to prevent desiccation and deformation. A concern in increment-core sampling is that the coring process may compress or deform the wood as the auger penetrates and the core is extracted. Manuals specify that the wood tissue near the bit can be compressed during drilling, and recent studies recognize core compaction as a bias in density estimates (Phipps 1985; Gao et al. 2017; Zhao et al. 2025). In the present study, this risk was minimized by employing sharp Pressler borers, carefully extracting cores at breast height, and immediately sealing them in tubes or straws to mitigate post-sampling distortion. All samples were conditioned to a uniform 12% EMC before testing, and volume was determined by water displacement for the Fractometer sections rather than relying solely on the nominal core diameter. Nevertheless, there is no direct experimental evidence within this dataset to confirm that compression or stretching during coring was absent; consequently, it is acknowledged as a potential source of bias and recognized as a limitation of the core-based density measurements.

Integrated sampling and specimen-preparation scheme for the two oak stands. (A) Tree-level sampling at breast height (L; 1.3 m) and below the crown base (H), including collection of logs and discs

Fig. 1. Integrated sampling and specimen-preparation scheme for the two oak stands. (A) Tree-level sampling at breast height (L; 1.3 m) and below the crown base (H), including collection of logs and discs. (B) Disc processing into 1-cm radial sections for dendrochronology. (C) Log processing into prisms. (D) Prism processing into boards and 20-mm sections. (E) Preparation of 20 × 20 × 300 mm standard test specimens (STS) for three-point bending. (F, G) Preparation of 10-mm-diameter increment cores (C10) into 1-cm sections for compression testing and density determination and 5-mm-diameter increment cores (C5) into five-tree-ring sections for Fractometer II testing and density determination. Red lines indicate cutting or marking positions; blue and green elements indicate specimens or discs/logs retained for the corresponding analyses.

Dendrochronology

Tree-ring analysis was performed on discs and cores. For Trees 1–6, discs were sectioned into 1-cm radial segments and sanded to 400-grit. For Trees 7–18, two 5-mm cores per tree were extracted and prepared in the same manner. Transverse sections were scanned at 1200 dpi using an HP Scanjet G4050 scanner. Tree-ring widths (TRW), earlywood (EW), and latewood (LW) proportions were measured with WinDendro 2009 Regular software (Regent Instruments Inc., Canada), and average TRW and LW curves were calculated in Microsoft Excel.

Density

Wood density was determined for all samples used in the mechanical property tests and Fractometer II testing. The specimens were acclimated to a moisture content of 12% (MC 12%). Three distinct sample types were included.

Sample 1

The dimensions of each STS specimen were measured in three anatomical directions to determine its volume, and its weight was recorded. The wood density of the specimens at MC 12% was calculated according to Eq. 1,

(1)

where ρ₁₂ denotes the wood density at MC 12 %, m₁₂ represents the weight of the sample (kg), and V₁₂ indicates the volume of the sample (m³).

Sample 2

C5 cores, designated for Fractometer II testing, were weighed. To determine their volume, the wood cores were submerged in water, and the displaced water was measured (Olesen 1971). Subsequently, the five-mm cores’ wood density (ρC5) was computed using Eq. 1 above. For Fractometer density determination, the broken core sections were weighed immediately after testing, and their volumes were determined by the Olesen (1971) soaking method at 12% EMC (Eq. 1).

Sample 3

C10 cores were sectioned along the radius into 10-mm cylinders. We measured the diameter and length with a digital calliper (accuracy 0.01 mm) and then calculated each cylinder’s volume. Ten-mm cores’ wood density (ρC10) and STS specimens’ wood density (ρSTS) were also determined using Eq. 1.

Mechanical Properties Testing

Mechanical tests were performed with standardized equipment and measurement methods (Merela and Čufar 2013; Bucur 2023). Bending strength attributes—modulus of rupture (MOR) and modulus of elasticity (MOE)—were measured with the Zwick Z050/TH 3A machine (Zwick GmbH & Co. KG, Ulm, Germany). Compression parallel to the grain was measured on core subsamples with the Tinius Olsen 10 ST machine (Tinius Olsen TMC, Horsham, PA, USA), which was selected because its 10 kN load cell provides improved force-measurement accuracy for the compression test. Although the maximum bending forces were similar (up to about 3500 N), bending tests used the Zwick machine because its clip-on deflectometers provide more precise deflection measurements than the Tinius Olsen’s crosshead measurement. The Tinius Olsen’s deflection readings are roughly an order of magnitude less accurate. As a result, the minor force measurement inaccuracies of the Zwick machine were considered negligible compared to the deflection measurement inaccuracies that would occur if bending were performed on the Tinius Olsen. Thus, the Tinius Olsen device was used solely for compression testing.

The IML Fractometer II (Instrumenta Mechanik Labor GmbH, Wiesloch, Germany) was employed for semi-destructive (forestwise) bending-shear evaluation of C5 cores to determine whether a portable device can generate results comparable to those of standard testing apparatus (Diaz-Maroto and Tahir 2019).

The statistical analyses comprised a two-sample Student’s t-test to assess differences between wood sections and stands, Pearson’s correlation coefficient to quantify relationships among the methods used, and linear regression to examine relationships between wood density and selected variables. For the correlation analysis, coefficients were computed from averages across all samples measured with the same method, whereas the TRW and LW were averaged across all sampled trees. Samples assigned to the same analytical comparison were sufficiently comparable in sampling position, moisture condition, specimen preparation, and measurement protocol that method-level averages could be compared without obvious systematic differences due to these factors. Because the correlation analysis used method-level averages rather than individual replicate observations, the resulting coefficients describe associations among aggregated method outputs and should not be interpreted as individual-tree correlations or as independent estimates based on the full nominal sample size. Homogeneity was assumed in this work.

Bending strength

Logs were cut into orthotropic blocks measuring 20 mm × 20 mm × 300 mm for three-point STS – standard bending tests. Specimens were labelled by stem radius and conditioned at 20 °C and 65% relative humidity to an equilibrium moisture content of 12%. Tests were performed with a 240 mm span and a loading rate of 10 mm/min. MOR and MOE were calculated in accordance with ČSN 490115 and ČSN 490116.

Compressive strength

Ten-mm cores (C10) conditioned under identical conditions were sectioned into 10-mm-long samples. Compressive strength (σC||) was measured with a Tinius Olsen 10ST machine, with specimens aligned with the longitudinal axis and loaded at 2 mm/min until the force was reduced by 40%. Each core was cut into cylindrical samples starting from the cambium side, labeled sequentially (A, B, C, D…). Before testing, specimens were positioned with a 10 N preload between the compression plates and aligned with the load. Force was applied at 2 mm/min until failure, recorded by a 10 kN load cell with 0.01 N accuracy. Displacement was measured via crosshead position with 0.1 µm accuracy.

Fractometer II – Bending strength

Five-mm diameter cores (C5) were conditioned under the same protocol. Lines were marked every five rings from the cambium side, and bending assessments were performed with a Fractometer II instrument. Bending strength (σb) and maximum bending angle (αb) were recorded.

Pre-test treatment and labelling: All wooden cores were conditioned for five months at 65% relative humidity and 20 °C to reach an equilibrium moisture content (EMC) of 12%. Using a stereo microscope, marks were then made on each core at five-tree-ring intervals with a permanent marker, beginning at the cambium side. These marks separated the core into sections labelled A, B, C, and so forth in the direction from the cambium toward the pith.

Testing: Each core was clamped in the IML Fractometer II so that the applied force acted in the direction of the wood fibres. The cores were broken at each section boundary (A, B, C, …). If a section was too short to be broken because of narrow tree-ring width, fracture was induced at the next section boundary. The maximum bending fracture strength was recorded in MPa together with the label of the section at which fracture occurred. The bending angle was also determined in degrees. This procedure was used to evaluate whether the portable Fractometer II could provide mechanical information comparable with measurements obtained using standard testing machines (Diaz-Maroto and Tahir 2019).

Table 3. Sample Preparation and Mechanical/dendrochronological Outputs for the Two Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand), under the Unified Protocol

Sample Preparation and Mechanical/dendrochronological Outputs for the Two Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand), under the Unified Protocol

RESULTS AND DISCUSSION

Growth, Density, and Mechanical Performance

The dendrochronological analysis showed differences in radial growth between the two sampled stands (Fig. 2). The SM stand (sessile oak upland stand), had a mean TRW of 149.85 ± 66.56 (0.01 mm) and LW proportion of 56.58 ± 11.02%, while the JA stand (English oak floodplain stand), had a higher mean TRW of 264.84 ± 77.74 (0.01 mm) and LW proportion of 64.84 ± 11.29% (Table 4). The mean number of tree rings at breast height DBH1.3 m was 99.8 ± 4.9 for the SM stand and 80.1 ± 5.3 for the JA stand, indicating different age and radial-growth characteristics in the two sampled stand–species combinations.

The TRW and LW chronologies showed similar interannual variation, indicating a shared regional growth signal. They differed in absolute growth levels and variability, consistent with the influence of regional climatic variability on oak growth, while differences in response amplitude may also reflect local stand conditions, tree characteristics, and the confounding of species and stand identity (Fritts 1976; Briffa and Osborn 1999; Hartl-Meier et al. 2015; Dobrovolný et al. 2016). Higher TRW in the JA stand material indicated faster radial growth than in the SM stand. LW data indicated that both stands sustained late-season tissue formation. Because LW influences tissue density and mechanical strength more than TRW alone, we considered these differences when interpreting the observed variation in mechanical behaviour (Wimmer 2002; Drew and Downes 2009; Vavrčík and Gryc 2012). This study demonstrated that chronology offers valuable context for wood properties; however, it is insufficient on its own to accurately predict mechanical performance. It must be evaluated alongside density and mechanical data.

Tree-ring width (TRW) and latewood proportion (LW) chronologies measured at breast height (BH1.3 m) for the two sampled stands: SM; sessile oak upland stand (Quercus petraea; dark grey line) and JA; English oak floodplain stand (Quercus robur; light grey line).

Fig. 2. Tree-ring width (TRW) and latewood proportion (LW) chronologies measured at breast height (BH1.3 m) for the two sampled stands: SM; sessile oak upland stand (Quercus petraea; dark grey line) and JA; English oak floodplain stand (Quercus robur; light grey line). The figure shows dendrochronological series obtained from discs and/or increment cores prepared for the unified sampling protocol; the plotted sample number is the number of measured samples contributing to each chronology.

Mechanical Properties and Density by Stand

The two sampled stands differed in mechanical properties and density, with SM representing the sessile oak upland stand and JA representing the English oak floodplain stand. The SM stand showed higher mean values for key mechanical parameters, including MOE (9176 ± 775 MPa), MOR (93.61 ± 6.05 MPa), Fractometer σb (20.56 ± 2.25 MPa), αb (12.38 ± 0.79°), and σC|| (27.37 ± 2.34 MPa).

SM stand density values ρSTS were 712.90 ± 37.16 kg/m³ for STS specimens, 729.77 ± 30.31 kg/m³ for 10-mm cores (ρC10), and 743.23 ± 45.03 kg/m³ for 5-mm cores (ρC5). These values fall within the range for mature European oak and match expected density and mechanical performance for sessile oak in Central Europe (Olarescu et al. 2016; Büyüksarı et al. 2017; Sejdiu et al. 2020; Nocetti et al. 2024). English oak trees (JA stand) had lower mean STS bending properties, with MOE of 8029 ± 684 MPa, MOR of 85.72 ± 7.82 MPa, Fractometer σb of 17.31 ± 1.94 MPa, and σC|| of 26.61 ± 1.38 MPa. These values, though lower than those of sessile oak trees (SM stand), remain suitable for structural hardwood (Gustafsson 2010; Gryc et al. 2025). The JA stand ρSTS values were 654.63 ± 37.35 kg/m³ for STS specimens, 726.98 ± 18.57 kg/m³ for ρC10, and 742.57 ± 32.14 kg/m³ for ρc5. These results show that the sampled SM material had higher density and bending strength than the sampled JA material, broadly consistent with previous reports of variation in oak density and mechanical properties among species and growing environments (Vavrčík and Gryc 2012; Eaton et al. 2016; Diaz-Maroto and Tahir 2018; Giagli et al. 2018); however, the present design cannot determine whether the observed differences reflect species, stand conditions, tree characteristics, or their combination.

Within stands, wood density increased from STS specimens to C10 and C5 cores, with significant differences between ρSTS and cores, but not between ρC10 and ρC5. This suggests the two core sizes provide similar density info, supporting core-based semi-destructive wood assessment (Schweingruber et al. 1978; Krauss et al. 2011; Terrasse et al. 2021; Gendvilas et al. 2024).

Table 4. Mean Values and Standard Deviations of the Measured Variables for the Two Sampled Stands, SM (sessile oak upland stand, Quercus petraea) and JA (English oak floodplain stand, Quercus robur)

Mean Values and Standard Deviations of the Measured Variables for the Two Sampled Stands, SM (sessile oak upland stand, Quercus petraea) and JA (English oak floodplain stand, Quercus robur)

Integrated Relationships among Mechanical Properties

Relationships among the mechanical properties differed between the two sampled stands (Table 5). In the SM stand, MOE and MOR were almost perfectly correlated (r=0.99), and σC|| was also strongly associated with both MOE (r=0.82) and MOR (r=0.79). In the JA stand, MOE and MOR again showed a very strong relationship (r=0.96), but σC|| showed little useful association with either MOE (r=-0.06) or MOR (r=-0.21).

The strong MOE-MOR relationship in both stands is fully consistent with established theory and empirical evidence indicating that stiffness and bending strength share structural determinants such as density, fiber organization, and cell-wall characteristics (Kollmann and Côté 1968; Baar et al. 2015; Collins et al. 2023). By contrast, the differing compression-bending relationships suggest that these traits were not coordinated in the same way across the two sampled materials. Because compression and bending failure depend on overlapping yet distinct anatomical controls, such variation in the correlation structure is biologically plausible (Cave 1968; Schniewind 1989; Almeida et al. 2023).

The Fractometer-derived σb showed little correlation with STS bending properties. In sessile oak, Fractometer σb showed negligible correlations with MOE and MOR (both r = -0.21), and in English oak, the correlations were similarly weak (both r = 0.03). This indicates the Fractometer output reflects a localized or method-specific aspect of mechanical response rather than serving as a direct substitute for MOE or MOR, consistent with previous findings that different testing configurations capture complementary, not interchangeable, information (Bodig and Jayne 1982; Büyüksarı et al. 2017; Diaz-Maroto and Tahir 2019).

Table 5. Correlation Coefficients among Mechanical, Density, and Dendrochronological Variables for the Two Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand)

Correlation Coefficients among Mechanical, Density, and Dendrochronological Variables for the Two Sampled Stands, SM (sessile oak upland stand) and JA (English oak floodplain stand)

 

The ab also showed consistently negative, though generally moderate, relationships with MOE and MOR in both stands. In sessile oak, the ab parameter correlated with MOE at r = -0.49 and with MOR at r = -0.48, whereas in English oak the corresponding values were r = -0.63 and r = -0.66. Although this pattern is directionally consistent with the expected adverse effect of grain deviation on load transfer and strength, the present results do not support ab as a primary predictor relative to density (Bergander and Salmén 2002; Gindl and Schöberl 2004; Koman et al. 2013).

Among all measured variables, density showed the clearest and most consistent relationship with bending performance. In the SM stand, ρSTS correlated very strongly with both MOE and MOR (r=0.96 for both), and ρC10 showed slightly stronger correlations with MOE and MOR (r=0.98 for both). The ρC5 showed weaker but still meaningful relationships with MOE and MOR (r=0.63 and r=0.64, respectively). Notwithstanding this potential bias, the density-estimation method employed herein remains justifiable for two primary reasons. First, the densities derived from cores were used primarily as screening variables and subsequently validated against standard-specimen density and mechanical properties within the same study design. Second, the discrepancy in stand-level standard-specimen density between SM and JA was 58.3 kg/m³, whereas the difference in mean ρC5 between stands was merely 0.7 kg/m³, with the within-stand standard deviations for core density ranging from 32 to 45 kg/m³. This pattern indicates that any deformation-related bias in the C5 cores is more likely to affect absolute values than to alter the principal conclusion that density is strongly associated with bending performance. Nonetheless, because recent research shows that increment-core methodologies can introduce species-specific systematic bias (Zhao et al. 2025)—particularly when cores are compared directly with reference blocks—the current core-density values should be regarded as operational estimates rather than unbiased, absolute measurements.

In the JA stand, ρSTS correlated highly with MOE (r=0.90) and MOR (r=0.98), while ρC10 also showed strong links with MOE (r=0.73) and MOR (r=0.83). The ρC5 had weaker but positive correlations: r=0.62 for MOE and r=0.71 for MOR. Density measures were highly related within stands: in SM, ρSTS and ρC10 core densities correlated at r=0.95; in JA, r=0.89. Core-based densities captured much of the same structural information as ρSTS, more so with ρC10 than ρC5. This aligns with the wood mechanics literature, which identifies density as a key predictor of stiffness and strength (Green et al. 1999; Baar et al. 2015; Nasir et al. 2021). The results affirm density as a primary screening variable for oak, though smaller cores may slightly reduce predictive accuracy when mean density is similar.

TRW and LW Proportion as Secondary Predictors

The dendrochronological variables were informative, but their predictive value differed between the two sampled stands. In the SM stand, TRW showed only weak-to-moderate correlations with MOE (r=0.35) and MOR (r=0.38), whereas the LW proportion showed stronger correlations with MOE (r=0.66) and MOR (r=0.68). This indicates that, in the SM stand material, the LW proportion was more closely related to mechanical quality than to radial growth rate alone. That pattern agrees with earlier studies showing that LW proportion often has a more direct structural connection to density and strength than total TRW, because it reflects the proportion of thicker-walled, mechanically important tissue (Vavrčík and Gryc 2012; Björklund et al. 2021; Torbenson et al. 2023). In the JA SM stand, both TRW and LW proportions were informative, but TRW was a stronger predictor of MOR and MOE, with correlations of r=0.85 and r=0.76, respectively. This result is consistent with the broader wood-science view that growth rate can influence wood quality by affecting the balance between EW and LW, although the strength and direction of that effect remain species- and site-dependent (Larson 1969; Zobel and Talbert 1984; Romagnoli et al. 2014). Carmona Uzcategui et al. (2020) reported similar species-level differences in clear-wood mechanical performance for red oak and white oak, where MOE and MOR differed between the two oak groups and were associated with density and LW characteristics.

The stronger TRW-LW association in JA (r=0.94) than in SM (r=0.76) suggests a more robust linkage between TRW and LW formation in the English oak material. A similar partial decoupling between TRW and LW-related variables has been documented in oak dendrochronology, where TRW and LW development may respond variably to seasonal environmental conditions (Souto-Herrero et al. 2018; Radaković and Stajić 2021; Vitali et al. 2022). Overall, the current findings show that dendrochronological variables can improve wood-quality interpretation; however, they do not consistently correlate with density across both study stands.

Comparative Analysis of Mechanical-Property Dependencies across the Two Sampled Stands

Density–strength relationships across sites

The regression analyses of MOR and MOE against ρSTS showed highly consistent patterns in both the SM and JA stands, despite their contrasting dendrochronological characteristics (Fig. 3). MOR exhibited exceptionally high coefficients of determination in both stand, and the regression lines were nearly identical in slope, indicating a strong and transferable density–strength relationship across these oak stands. This pattern is consistent with research showing that wood density is a primary determinant of mechanical properties across hardwood species and growth conditions (Olarescu et al. 2016; You et al. 2021; Nasir et al. 2021; Gryc et al. 2025).

Similar slopes suggest that the underlying mechanism linking MOR to density operates in much the same way in both stands, namely, through the amount of cell-wall material per unit volume that contributes to bending resistance. MOE also showed high coefficients of determination in both stands, although the relationship was slightly less uniform than for MOR. This difference is consistent with MOE’s greater sensitivity to microscopic structural features such as microfibril angle and cell-wall thickness gradients (Bergander and Salmén 2002; Gindl and Schöberl 2004).

From a practical standpoint, these findings indicate that semi-destructive density measurements from increment cores can predict bending properties across both stands with limited need for site-specific recalibration. This interpretation is supported by emerging work on portable resistance-drilling and other field-based wood-quality methods, which similarly identify density as a robust predictor of mechanical performance (Gendvilas et al. 2024, 2025).

Compression strength divergence

A clearer stand-specific difference emerged in the relationships between bending properties MOR, MOE, and σC|| (Fig. 4). In the SM stand, MOR and σC|| were substantially correlated, whereas in the JA stand, no detectable correlation was observed. This divergence suggests that mechanical properties were more tightly coordinated in the SM stand wood, while the JA stand material showed greater independence between bending and compression behavior.

Relationships between STS density (ρSTS) and bending properties in the two sampled stands: SM = sessile oak upland stand (Quercus petraea) and JA = English oak floodplain stand (Quercus robur).

Fig. 3. Relationships between STS density (ρSTS) and bending properties in the two sampled stands: SM = sessile oak upland stand (Quercus petraea) and JA = English oak floodplain stand (Quercus robur). The figure shows regression relationships between modulus of rupture (MOR) and ρSTS, and between modulus of elasticity (MOE) and ρSTS, based on standard test specimens prepared from felled trees in each stand.

This difference between the two sampled stand–species combinations may reflect variation in wood ultrastructure and growth conditions (Pretzsch et al. 2013; Heklau et al. 2019; Fontes et al. 2022; Gryc et al. 2025; Móricz et al. 2025), although the present design does not allow the responsible factors to be distinguished. In the SM stand, STS bending and σC|| appear to covary more closely, implying a more integrated mechanical organization of the wood. In the JA stand, by contrast, the absence of an MOR/σC|| relationship suggests that distinct failure mechanisms may contribute to the observed relationship in the JA material.

The result has direct implications for timber assessment because it shows that σC|| cannot be inferred reliably from bending behavior alone across both sites. Predicting compression-related performance may require additional structural variables, such as wall-thickness ratios, microfibril angle, or three-dimensional fibre orientation, rather than a single bivariate model (Leijten 2002; Wu et al. 2023). This also aligns with machine-learning studies showing that more complex models often outperform simple linear regression when heterogeneous failure mechanisms control wood properties (Khan et al. 2025).

Relationships between compression strength parallel to grain (σC||) measured on C10 increment cores and bending properties measured on STS specimens in the two sampled stands

Fig. 4. Relationships between compression strength parallel to grain (σC||) measured on C10 increment cores and bending properties measured on STS specimens in the two sampled stands: SM; sessile oak upland stand (Quercus petraea) and JA; English oak floodplain stand (Quercus robur). The figure shows MOR versus σC|| and MOE versus σC|| for the unified sampling design.

Grain angle and anisotropy

The analysis revealed no significant correlation between αb and either MOR or MOE in either stand (Fig. 5).

Relationships between Fractometer maximum bending angle (αb) measured on C5 increment cores and bending properties measured on STS specimens in the two sampled stands

Fig. 5. Relationships between Fractometer maximum bending angle (αb) measured on C5 increment cores and bending properties measured on STS specimens in the two sampled stands: SM; sessile oak upland stand (Quercus petraea) and JA; English oak floodplain stand (Quercus robur). The figure shows MOR versus αb and MOE versus αb under the unified sampling protocol.

This contrasts with literature reporting strong grain-angle effects on wood stiffness and strength (Güntekin et al. 2016; Ozyhar et al. 2016; Collins et al. 2023). However, the grain deviations measured here were modest, and stiffness losses are less pronounced within a limited angle range than at larger deviations from the longitudinal axis (Roszyk et al. 2010).

Local variability in grain angle, including microfibril-angle variation and spiral grain, may also have introduced enough noise to obscure any simple bivariate relationship (Diaz-Maroto and Tahir 2018; Arriaga et al. 2023). In this sense, the present results highlight the difference between local grain deviations measured in individual specimens and the integrated influence of fibre orientation across a whole cross-section (Bratu et al. 2025). More advanced approaches, such as digital image correlation and three-dimensional stress mapping, suggest that grain-angle effects become clearer when stress concentration and failure initiation are explicitly modeled rather than averaged across the bulk material (Xie et al. 2020; Tamke et al. 2025).

Tree-ring variables as predictors

The regression analyses between dendrochronological variables and mechanical properties showed differences between the two stands. In addition, there was a shared pattern of useful predictive value for both TRW and LW proportion (Fig. 6). In both stands, MOR and MOE were related to TRW, although the strength and clarity of these relationships varied by site. This agrees with earlier work showing that radial growth rate reflects coordinated changes in cell size and wall thickness, with faster growth generally producing more EW and thinner-walled tissue (Romagnoli et al. 2014; Sochová et al. 2021).

Relationships between dendrochronological variables and bending properties in the two sampled stands: SM = sessile oak upland stand (Quercus petraea) and JA = English oak floodplain stand (Quercus robur). Fig. 6. Relationships between dendrochronological variables and bending properties in the two sampled stands: SM = sessile oak upland stand (Quercus petraea) and JA = English oak floodplain stand (Quercus robur). The figure shows modulus of rupture (MOR) and modulus of elasticity (MOE) plotted against tree-ring width (TRW) and latewood proportion (LW), using the dendrochronological samples linked to the unified stand-level sampling design.

LW proportion showed the strongest and most consistent relationships with mechanical properties across both stands. This is biologically plausible because LW cells have thicker walls, smaller lumens, and greater stiffness and strength per unit volume than EW cells (Büyüksarı et al. 2018). As a result, LW proportion captures the fraction of mechanically superior tissue more directly than TRW alone, which explains its stronger correlations with MOR and MOE (Muñoz 2025). Previous studies similarly showed that TRW components in English oak respond to climatic conditions in a site-dependent manner, supporting the view that TRW and related growth traits should be interpreted as complementary rather than universal predictors of wood quality (Gričar et al. 2013; Roibu et al. 2020). This interpretation is further supported by studies showing that radial density gradients integrate multiple structural factors and often outperform simple growth metrics in predicting mechanical performance (Torbenson et al. 2023; Jiang et al. 2024; Lozjanin et al. 2024).

The stand-specific differences in property correlations, especially the presence or absence of the MOR–compression relationship, fit broader patterns known from dendroecology and wood science. Studies of sessile oak across Central Europe show that growth responses and wood-property development are strongly site-dependent, with dry upland sites and wetter environments producing different structural and mechanical outcomes (Rybníček et al. 2015; Andrzejczyk et al. 2024). In upland sessile oak, moderate water limitation tends to favor denser wood formation, thicker fibre walls, and smaller vessels, all of which improve mechanical performance (Vavrčík and Gryc 2012; Giagli et al. 2018; Diaz-Maroto and Tahir 2018; Březina et al. 2020).

The observed pattern of wood formation helps interpret differences between the two sampled stand materials. In the SM stand, continuous LW thickening likely formed a more uniform wall structure and a better balance between stiffness and strength. A lower LW proportion indicates a shorter LW window, possibly due to drought, which can limit wall thickening and weaken compression performance (Bendtsen 1978; Fengel and Wegener 1989). In the JA stand, the lower LW proportion is consistent with a shorter LW-formation window in the sampled material, a pattern that may be associated with the contrasting stand conditions but is not directly tested here. These trends are consistent with the sampled English oak floodplain material, but they should not be interpreted as a direct test of species-level ecological strategy within the present design.

Practical Implications and Limitations

In both stands, density measured from STS specimens and increment cores was strongly associated with MOE and MOR, indicating that density-based screening can assess oak timber quality without extensive destructive testing (Brashaw et al. 2009; Gendvilas et al. 2024; Seidl et al. 2024; Uldry et al. 2024). Validation across additional stands and species combinations is required before broader generalisation.

The transferability of density-strength relationships across the two sampled stands contrasted with the stronger stand-associated variation observed for compression strength. Because the instruments measured different properties on different specimen types, Fractometer outputs were interpreted as complementary indicators rather than direct replacements for Zwick MOR/MOE or Tinius Olsen compression results. European grading systems are based primarily on visual assessment and ultrasonic or stress-wave techniques that reflect elastic properties (EN 1912 2012; EN 338 2016; Nocetti et al. 2024; Uldry et al. 2024). In this context, the present results indicate that density, obtained by destructive or semi-destructive methods, reliably predicts bending performance across oak stands without extensive stand-specific calibration. In contrast, simple bivariate relationships did not adequately capture compression strength, suggesting that this property depends more strongly on local anatomical and structural features. For that reason, methods such as resistance drilling or Pilodyn may be more suitable when the objective is to characterize tissue structure or cell-wall-related variation (Gafenco et al. 2024; Seidl et al. 2024; Seiwald et al. 2024). Whether this relationship transfers to other stands or species requires testing with a design that includes replicated species and stand conditions.

Density-based screening was the most robust practical approach for evaluating wood quality in the sampled material. Both standard-specimen density and increment-core density showed strong relationships with bending properties, which supports the use of non-destructive and semi-destructive methods in forestry and timber grading (Brashaw et al. 2009; Gendvilas et al. 2024; Seidl et al. 2024; Uldry et al. 2024). The C10 cores gave the most consistent results, but C5 cores showed similar mean density values and still captured the principal trends. This indicates that smaller cores may be used for minimally invasive preliminary screening when material preservation is important (Gendvilas et al. 2024; Seidl et al. 2024).

Dendrochronological variables provided supplementary interpretation of variation in wood properties. LW proportion was consistently related to bending properties in both stands, whereas TRW was more informative in the English oak material. These results indicate that growth traits can improve the interpretation of differences associated with the sampled stand conditions when considered alongside density, but they were less robust than density as a standalone predictor (Friedrich et al. 2004; Sochová et al. 2021; Torbenson et al. 2023). The observed relationships also suggest that dendrochronological analysis may provide a low-cost, minimally invasive option for timber quality assessment in reclaimed or heritage materials, where destructive sampling is restricted (Rybníček et al. 2015; Sochová et al. 2021).

The two stands also differed in the internal coordination of their mechanical traits. In the SM stand, MOE, MOR, and compression strength were strongly interrelated, whereas in JA, compression strength showed little association with bending properties. This result indicates that bending and compression behavior did not show the same relationships across the two sampled stands and that a single universal predictive model is unlikely to describe all properties equally well (Spiecker et al. 1996; Vavrčík and Gryc 2012). The strong MOE-MOR relationships observed in both stands are consistent with the shared anatomical basis of stiffness and bending strength, including density, fiber organization, and cell-wall characteristics (Kollmann and Côté 1968; Baar et al. 2015; Collins et al. 2023).

The Fractometer-derived parameters were less directly related to standard bending properties than density. Although the grain-angle parameter showed directionally consistent negative relationships with MOE and MOR, its predictive value was lower than that of density. This suggests that Fractometer outputs reflect a more localized or method-specific aspect of mechanical response and should be interpreted as complementary rather than interchangeable with standard strength measurements (Bodig and Jayne 1982; Büyüksarı et al. 2017; Diaz-Maroto and Tahir 2019). In practical terms, the findings support a tiered assessment approach in which density and LW proportion are used for initial screening, whereas compression-related properties are measured or modeled separately when they are critical for the intended use.

The agreement between standard-specimen density relationships and core-derived density measurements supports using semi-destructive sampling for in-situ wood quality assessment. Strong MOR-density relationships in both stands indicate that increment-core methods are suitable for field-based screening (Batista et al. 2023). However, the greater variability of some MOE relationships indicates that elastic-modulus prediction remains sensitive to methodological differences and therefore requires careful standardization when destructive and non-destructive approaches are compared.

These findings indicate that validation against reference mechanical testing remains necessary before practical deployment, as required by standards such as BS EN 408 (1995). A tiered strategy is therefore appropriate, with density and LW metrics used for screening and compression-related properties evaluated separately when they are important for structural performance.

Comparison of the SM and JA stands revealed both general and stand-specific aspects of oak wood mechanics. Density-bending relationships were highly consistent across stands, which supports their use in predictive models for oak timber (Römer et al. 2025). In contrast, compression strength, grain-angle effects, and the internal coordination of mechanical properties were more stand-dependent, indicating that no single model can capture all relevant properties with equal accuracy.

A more robust framework should therefore combine broadly transferable predictors, such as density, with stand-sensitive descriptors, including LW proportion and other structural variables. Future work should extend this approach by incorporating anatomical features, fiber-orientation data, and non-destructive imaging into multivariate or machine-learning models, which are increasingly effective when failure mechanisms are complex and heterogeneous (Barnett and Jeronimidis 2003; Walker 2006; Khan et al. 2025).

CONCLUSIONS

  1. Wood density was found to be the strongest and most consistent predictor of bending performance in both oak stands, and both standard-specimen density and core-based density showed strong positive relationships with modulus of elasticity (MOE) and modulus of rupture (MOR).
  2. Sessile oak (Quercus petraea) (SM), the upland stand, showed higher mean density, MOE, and MOR than English oak (Quercus robur) (JA), the floodplain stand, indicating clear differences in wood quality between the two sampled stands.
  3. Density relationships with bending properties were broadly transferable across the two sampled stands, whereas compression strength showed stronger stand-associated variation and could not be explained adequately by simple bivariate models.
  4. The 10-mm increment cores gave the most consistent predictions of mechanical performance, while Fractometer 5-mm cores remained suitable for minimally invasive preliminary screening; LW proportion provided useful supplementary information but was less consistent than density.
  5. The present sampling design supports comparison between two contrasting sampled stand-species combinations, but it does not support independent inference about ecological effects separate from species and stand.

ACKNOWLEDGMENTS

The authors are grateful for the support of the Czech Science Foundation (Grant No. 24-14324L). The work of LK was funded by the European Union, contract no. 0005-404, Recovery and Resilience Facility (NOO) and “NextGenerationEU”. The research programme P4-0430 (ARIS) provided additional support.

Conflict of Interest

No conflict.

Use of Generative AI

The Authors used GRAMMARLY PRO for spelling and grammar proofreading of the article. No Generative AI was used to prepare images, figures, graphs, or diagrams.

REFERENCES CITED

Almeida, J. P. B., Wolenski, A. R. V., Rodrigues, E. F. C., de Araujo, V. A., Panzera, T. H., de Campos, C. I., Molina, J. C., Christoforo, A. L., and Lahr, F. A. R. (2023). “Characteristic strengths in the compression and in the static bending as parameters to estimate characteristic shear strength for timber design,” Revista Árvore 47, article e4708. https://doi.org/10.1590/1806-908820230000008

Andrzejczyk, T., Liziniewicz, M., and Bolibok, L. (2024). “Growth and quality of 16-year-old sessile oak (Quercus petraea (Matt.) Liebl.) planted in traditional and alternative row planting patterns,” Forestry: An International Journal of Forest Research 97(4), 564-579. https://doi.org/10.1093/forestry/cpad059

Arriaga, F., Wang, X., Llana, D. F., Esteban, M., and Niemz, P. (2023). “Mechanical properties of wood: A review,” Forests 14(6), article 1202. https://doi.org/10.3390/f14061202

Arenas-Navarro, M., Oyama, K., García-Oliva, F., Torres-Miranda, A., de la Riva, E.G., and Terrazas, T. (2021). “The role of wood anatomical traits in the coexistence of oak species along an environmental gradient,” AoB PLANTS 13(6), 1-14. https://doi.org/10.1093/aobpla/plab066

Baar, J., Tippner, J., and Rademacher, P. (2025). “Prediction of mechanical properties – Modulus of rupture and modulus of elasticity of five tropical species by nondestructive methods,” Maderas. Ciencia Y Tecnología 17(2), 239-252. https://revistas.ubiobio.cl/index.php/MCT/article/view/1200

Barnett, J. R., and Jeronimidis, G. (2003). Wood Quality and Its Biological Basis, Blackwell Publishing, Oxford, UK.

Batista, M., Amorim, A., Lopes Silva, D. A., Aquino, V., Lahr, F. A. R., and André Luis Christoforo, A. (2023). “Representativeness of the fiber parallel elasticity modulus value referring to the Brazilian standard C40 strength class in the design of timber structures,” Forestry Science- Cienc. Rural 53(3). https://doi.org/10.1590/0103-8478cr20210289

Bendtsen, B. A. (1978). “Properties of wood from improved and intensively managed trees,” Forest Products Journal 28(10), 61-72.

Bergander, A., and Salmén, L. (2002). “Cell wall properties and their effects on the mechanical properties of fibers,” Journal of Materials Science 37, 151-156. https://doi.org/10.1023/A:1013115925679

Björklund, J., Seftigen, K., Schweingruber, F., Fonti, P., Bryukhanova, M. V., Cuny, H. E., Carrer, M., Castagneri, D., and Frank, D. C. (2017). “Cell size and wall dimensions drive distinct variability of earlywood and latewood density in Northern Hemisphere conifers,” New Phytologist 216(3), 728-740. https://doi.org/10.1111/nph.14639

Björklund, J., Von Arx, G., Fonti, P., Stridbeck, P., De Mil, T., Neycken, A., and Seftigen, K. (2021). “The utility of bulk wood density for tree-ring research,” Dendrochronologia 69, article 125880. https://doi.org/10.1016/j.dendro.2021.125880

Bodig, J., and Jayne, B. A. (1982). Mechanics of Wood and Wood Composites, Van Nostrand Reinhold, New York.

Bölöni, J., Aszalós, R., Frank, T., and Ódor, P. (2021). “Forest type matters: Global review about the structure of oak dominated old-growth temperate forests,” Forest Ecology and Management 500, article 119629. https://doi.org/10.1016/j.foreco.2021.119629

Bose, A. K., Scherrer, D., Camarero, J. J., Ziche, D., Babst, F., Bigler, C., Bolte, A., Dorado-Linan, I., Etzold, S., … and Rigling, A. (2021). “Climate sensitivity and drought seasonality determine post-drought growth recovery of Quercus petraea and Quercus robur in Europe,” Science of the Total Environment 784, article 147222. https://doi.org/10.1016/j.scitotenv.2021.147222.

Bratu, I., Dinca, L., Constandache, C., and Murariu, G. (2025). “Resilience and decline: The impact of climatic variability on temperate oak forests,” Climate 13(6), article 119. https://doi.org/10.3390/cli13060119

Briffa, K. R., and Osborn, T. J. (1999). “Seeing the wood from the trees,” Science 284(5416), 926-927. https://doi.org/10.1126/SCIENCE.284.5416.926

Brashaw, B. K., Bucur, V., Divos, F., Goncalves, R., Lu, J., Meder, R., Pellerin, R. F., Potter, S., Ross, R. J., Wang, X., and Yin, Y. (2009). “Nondestructive testing and evaluation of wood: A worldwide research update,” Forest Products Journal 59(3), 7-14.

Březina, D., Kadavý, J., Kneifl, M., and Michal, J. (2020). “Comparison of economic efficiency of management systems with prevailing representation of sessile oak (Quercus petraea (Matt.) Liebl.) in the territory of Křivoklátsko Forest Park (Czech Republic),” Forests 11(4), article 447. https://doi.org/10.3390/f11040447

BS EN 408 (1995). “Timber structures – Structural timber and glued laminated timber – Determination of some physical and mechanical properties,” European Committee for Standardisation, Brussels.

Bucur, V. (2023). “A review on acoustics of wood as a tool for quality assessment,” Forests 14(8), article 1545. https://doi.org/10.3390/f14081545

Büyüksarı, Ü. (2017). “Effect of loading rate on mechanical properties of micro-sized oak wood,” Maderas. Ciencia y Tecnología 19(2), 163-172. https://doi.org/10.4067/S0718-221X2017005000014

Büyüksarı, Ümit, As, N., Dündar, T., and Korkmaz, O. (2017). “Micro-mechanical properties of oak wood and comparison with standard-sized samples,” Maderas, Ciencia y Tecnología, 19(4), 481-494. https://doi.org/10.4067/S0718-221X2017005000801

Büyüksarı, Ü., As, N., and Dündar, T. (2018). “Intra-ring properties of earlywood and latewood sections of sessile oak (Quercus petraea) wood,” BioResources 13(1), 836-845. https://doi.org/10.15376/biores.13.1.836-845

Carmona Uzcategui, M. G., Seale, R. D., and Nistal França, F. J. (2020). “Physical and mechanical properties of clear wood from red oak and white oak,” BioResources 15(3), 4960-4971. https://doi.org/10.15376/biores.15.3.4960-4971

Cave, I. D. (1968). “The anisotropic elasticity of the plant cell wall,” Wood Science and Technology 2(4), 268-278. https://doi.org/10.1007/BF00350273

Cienciala, E., Apltauer, J., Exnerová, Z., and Tatarinov, F. (2008). “Biomass functions applicable to oak trees grown in Central-European forestry,” Journal of Forest Science 54(3), 109-120. https://doi.org/10.17221/2906-JFS

Collins, S., Jaaranen, J., and Fink, G. (2023). “Modelling the effect of three-dimensional grain angle on the tension strength of birch wood,” in: 13th World Conference on Timber Engineering, WCTE 2023, Oslo, Norway, pp. 428-434. Curran Associates Inc. https://doi.org/10.52202/069179-0058

ČSN 490115 (1979). “Wood. Determination of ultimate strength in flexure tests,” Czech Office for Standards, Metrology and Testing, Praha

ČSN 490116 (1982). “Wood. Determination of the modulus of elasticity in static bending,” Czech Office for Standards, Metrology and Testing, Praha

Diaz-Maroto, I. J., and Tahir, S. (2018). “Testing of wood physical properties in oak species (Quercus robur L., Q. petraea (Matts) Liebl. and Q. pyrenaica Willd.) for cooperage. Part II: wood grain,” Wood Research 63(6), 959-970.

Diaz-Maroto, I. J., and Tahir, S. (2019). “Test of wood properties in oak species (Quercus robur L., Quercus petraea (Matts) Liebl. and Quercus pyrenaica Willd.) for wine aging. Part III: porosity versus void ratio,” Wood Research 64(5), 833-846.

Ding, Z., Li, R., O’Connor, P., Zheng, H., Huang, B., Kong, L., Xiao, Y., Xu, W., and Ouyang, Z. (2021). “An improved quality assessment framework to better inform large-scale forest restoration management,” Ecological Indicators 123, article 107370. https://doi.org/10.1016/j.ecolind.2021.107370

Dobrovolný, L. (2014). “Potential of natural regeneration of Quercus robur L. in floodplain forests in the southern part of the Czech Republic,” Journal of Forest Science 60(12), 534-539. https://doi.org/10.17221/83/2014-JFS

Dobrovolný, L., Martiník, A., Drvodelić, D., and Oršanić, M. (2017). “Structure, yield and acorn production of oak (Quercus robur L.) dominated floodplain forests in the Czech Republic and Croatia,” South-east European Forestry 8(2), 127-136. https://doi.org/10.15177/seefor.17-18

Dobrovolný, P., Rybníček, M., Büntgen, U., Trnka, M., Brázdil, R., Stachoň, Z., Prokop, O., and Kolář, T. (2016). “Recent growth coherence in long-term oak (Quercus spp.) ring width chronologies in the Czech Republic,” Climate Research 70, 133-141. https://doi.org/10.3354/cr01402

Drew, D. M., and Downes, G. M. (2009). “The use of precision dendrometers in research on daily stem size and wood property variation: A review,” Dendrochronologia 27(2), 159-172. https://doi.org/10.1016/j.dendro.2009.06.008

Eaton, E., Caudullo, G., Oliveira, S., and de Rigo, D. (2016). “Quercus robur and Quercus petraea in Europe: Distribution, habitat, usage and threats,” in J. San-Miguel-Ayanz, D. de Rigo, G. Caudullo, T. Houston Durrant, and A. Mauri (eds.), European Atlas of Forest Tree Species, Publication Office of the European Union, Luxembourg, pp. 1-4.

EN 338 (2016). “Structural timber – Strength classes,” European Committee for Standardization, Brussels.

EN 1912 (2012). “Structural timber – Grading classes – Assignment of visual grades and species,” European Committee for Standardization, Brussels.

Fengel, D., and Wegener, G. (1989). Wood – Chemistry, Ultrastructure, Reactions, 2nd Ed., Walter de Gruyter, Berlin.

Fontes, C. G., Pinto-Ledezma, J., Jacobsen, A. L., Pratt, R. B., and Cavender-Bares, J. (2022). “Adaptive variation among oaks in wood anatomical properties is shaped by climate of origin and shows limited plasticity across environments,” Functional Ecology 36(2), 326-340. https://doi.org/10.1111/1365-2435.13964

Friedrich, M., Remmele, S., Kromer, B., et al. (2004). “The 12,460-Year Hohenheim Oak and pine tree-ring chronology from Central Europe – A unique annual record for radiocarbon calibration and paleoenvironment reconstructions,” Radiocarbon 46(3), 1111-1122. https://doi.org/10.1017/S003382220003304X

Fritts, H. C. (1976). Tree Rings and Climate, Academic Press, London.

Gafenco (Pleșca), I. M., Dinulică, F., Pleșca, B. I., and Șofletea, N. (2024). “Links between tree phenology and wood traits in sessile oak (Quercus petraea (Matt.) Liebl.),” Annals of Forest Research 67(2), 31-50. https://doi.org/10.15287/afr.2024.3364

Gao, S., Wang, X., Wiemann, M. C., Brashaw, B. K., Ross, R. J., and Wang, L. (2017). “A critical analysis of methods for rapid and nondestructive determination of wood density in standing trees,” Annals of Forest Science 74, 27. https://doi.org/10.1007/s13595-017-0623-4

Gendvilas, V., Lee, D. J., Kain, D. P., Kumar, C., Downes, G. M., Lausberg, M., and Harrington, J. J. (2024). “Predicting wood density using resistance drilling: The effect of instrument and operator,” Forests 15(1), article 157. https://doi.org/10.3390/f15010157

Gendvilas, V., Lee, D. J., Downes, G. M., Lausberg, M., and Harrington, J. J. (2025). Predicting wood properties using resistance drilling: The effect of needle diameter and battery,” Wood Material Science & Engineering 1-11. https://doi.org/10.1080/17480272.2025.2565371

Giagli, K., Baar, J., Fajstavr, M., Gryc, V., and Vavrčík, H. (2018). “Tree-ring width and variation of wood density in Fraxinus excelsior L. and Quercus robur L. growing in floodplain forests,” BioResources 13(1), 804-819. https://doi.org/10.15376/biores.13.1.804-819

Gindl, W., and Schöberl, T. (2004). “The significance of the elastic modulus of wood cell walls obtained from nanoindentation measurements,” Composites Part A: Applied Science and Manufacturing 35(11), 1345-1349. https://doi.org/10.1016/j.compositesa.2004.04.002

Green, D. W., Winandy, J. E., and Kretschmann, D. E. (1999). “Mechanical properties of wood,” in: The Chemistry of Solid Wood, R. M. Rowell (Ed.), American Chemical Society, Washington, DC, pp. 283-323.

Gričar, J., de Luis, M., Hafner, P., and Levanič, T. (2013). “Anatomical characteristics and hydrologic signals in tree-rings of oaks (Quercus robur L.),” Trees 27, 1669-1680. https://doi.org/10.1007/s00468-013-0914-9

Gryc, V., Giagli, K., Mikhailov, S., Stojanović, M., Tsalagkas, D., Vavrčík, H., and Horáček, P. (2025). “Variation in wood density between mature sessile oak and English oak trees growing in different vegetation zones,” Journal of Forest Science 71(12), 614-623. https://doi.org/10.17221/74/2025-JFS

Güntekin, E., Yılmaz Aydın, T., and Niemz, P. (2016). “Some orthotropic mechanical properties of Sessile oak (Quercus petraea) as influenced by moisture content,” Eurasian Journal of Forest Science 4(1), 40-47. https://doi.org/10.31195/ejejfs.258624

Gustafsson, S.I. (2010). “The strength properties of Swedish oak and beech,” Drewno 53(183), 67-83.

Hartl-Meier, C., Zang, C., Büntgen, U., Esper, J., Rothe, A., Göttlein, A., Dirnböck, T., and Treydte, K. (2015). “Uniform climate sensitivity in tree-ring stable isotopes across species and sites in a mid-latitude temperate forest,” Tree Physiology 35(1), 4-15. https://doi.org/10.1093/treephys/tpu096

Heklau, H., Jetschke, G., Bruelheide, H., Seidler, G., and Haider, S. (2019). “Species-specific responses of wood growth to flooding and climate in floodplain forests in Central Germany,” iForest 12, 226-236. https://doi.org/10.3832/ifor2845-012

Hietz, P., Rungwattana, K., Scheffknecht, S., and George, J. P. (2022). “Effects of provenance, growing site, and growth on Quercus robur wood anatomy and density in a 12-year-old provenance trial,” Frontiers in Plant Science 13, 795941. https://doi.org/10.3389/fpls.2022.795941

Hirofumi, I., Hirofumi, N., and Hideo, K. (2007). “Comparison between compression strength perpendicular to the grain and shear strength parallel to the grain of Western hemlock lumber,” Bulletin of FFPRI 6(1), 71-76.

Jiang, T., Feng, X., Xia, Z., Deng, S., and Wang, X. (2024). “Gradient variation and correlation analysis of physical and mechanical properties of moso bamboo (Phyllostachys edulis),” Materials 17(9), article 2069. https://doi.org/10.3390/ma17092069

Jönsson, M., Hekkala, A., Clemmensen, K., Kyaschenko, J., Kärvemo, S., Mielke, L., Sjögren, J., and Strengbom, J. (2025). “Inter-observer reliability in forest conservation value assessments,” Forest Ecology and Management 595, article 123006. https://doi.org/10.1016/j.foreco.2025.123006

Khan, T., Hasan, K., Hossen, M., Karim, M. F., and Khan, A. H. (2025). “Machine learning for predicting the mechanical properties of composite materials: A comparison of ensemble methods and analytical models,” EJSMT 1(6), 142-157. https://doi.org/10.59324/ejsmt.2025.1(6).13

Koman, S., Feher, S., Abraham, J., and Taschner, R. (2013). “Effect of knots on the bending strength and the modulus of elasticity of wood,” Wood Research 58(4), 617-626.

Kollmann, F. F., and Côté, W. A. (1968). Principles of Wood Science and Technology: I. Solid Wood, Springer-Verlag, Berlin. https://doi.org/10.1007/978-3-642-87928-9

Krauss, A., Moliński, W., Kúdela, J., and Čunderlík, I. (2011). “Differences in the mechanical properties of early and latewood within individual annual rings in dominant pine tree (Pinus sylvestris L.),” Wood Research 56(1), 1-12.

Larson, P. R. (1969). Wood Formation and the Concept of Wood Quality, Yale School of the Environment Bulletin 74, Yale University, New Haven, CT, USA.

Leijten, A. J. M. (2002). “Splitting strength of beams loaded by connections – Model comparison,” in: Proceeding of the International Council for Research and Innovation in Building and Construction, CIB-W18, Meeting Thirty-Five, Kyoto, Japan, paper 35-7-7).

Llana, D. F., Short, I., and Harte, A. M. (2020). “Use of non-destructive test methods on Irish hardwood standing trees and small-diameter round timber for prediction of mechanical properties,” Annals of Forest Science 77, 62. https://doi.org/10.1007/s13595-020-00957-x

Löf, M., Brunet, J., Filyushkina, A., Lindbladh, M., Skovsgaard, J. P., and Felton, A. (2016). “Management of oak forests: striking a balance between timber production, biodiversity and cultural services,” International Journal of Biodiversity Science, Ecosystem Services & Management 12(1-2), 59-73. https://doi.org/10.1080/21513732.2015.1120780

Lozjanin, R., Jokanović, D., Nikolić Jokanović, V., Živanović, K., Desimović, I., and Marinković, M. (2024). “Anatomical characteristics and assessment of wood fibers quality of mature pedunculate oak (Quercus robur L.) trees grown in different environmental conditions,” South-east European Forestry 15(1), 51-57. https://doi.org/10.15177/seefor.24-05

Mäkelä, A., Grace, J.C., Deckmyn, G., Kantola, A., and Campioli, M. (2010). “Simulating wood quality in forest management models,” Forest Systems 19(SI), 48-68. https://doi.org/10.5424/fs/201019S-9314

May, N., Guenther, E., and Haller, P. (2017). “Environmental indicators for the evaluation of wood products in consideration of site-dependent aspects: A review and integrated approach,” Sustainability 9(10), article 1897. https://doi.org/10.3390/su9101897

Merela, M., and Čufar, K. (2013). “Density and mechanical properties of oak sapwood versus heartwood,” Drvna Industrija 64(4), 323-334. https://doi.org/10.5552/drind.2013.1325

Móricz, N., Mészáros, I., Illés, G. Z., Garamszegi, B., Eötvös, C. B., Kern, A., Hirka, A., Berki, I., Borovics, A., Hollós, R., and Németh, T. M. (2025). “Radial growth projections reveal site-specific futures of different oak species with contrasting water availability in SW Hungary,” Frontiers in Forests and Global Change 8, article 1581222. https://doi.org/10.3389/ffgc.2025.1581222

Mölder, A., Meyer, P., and Nagel, R. (2019). “Integrative management to sustain biodiversity and ecological continuity in Central European temperate oak (Quercus robur, Q. petraea) forests: An overview,” Forest Ecology and Management 437, 324-339. https://doi.org/10.1016/j.foreco.2019.01.006

Muñoz, G. R. (2025). “Ring width distribution as a valuable anatomical trait for predicting bending strength and rigidity in European oak wood beams,” Canadian Journal of Forest Research 55, 1-10. https://doi.org/10.1139/cjfr-2024-0165

Nasir, V., Fathi, H., Fallah, A., Kazemirad, S., Sassani, F., and Antov, P. (2021). “Prediction of mechanical properties of artificially weathered wood by color change and machine learning,” Materials 14(21), article 6314. https://doi.org/10.3390/ma14216314

Nocetti, M., Aminti, G., Vicario, M., and Brunetti, M. (2024). “Mechanical properties of ancient wood structural elements assessed by visual and machine strength grading,” Construction and Building Materials 411, article 134418. https://doi.org/10.1016/j.conbuildmat.2023.134418

Nosenko, T., Schroeder, H., Zimmer, I., Buegger, F., Orgel, F., Burau, I., Padmanaban, P. B. S., Ghirardo, A., Bracker, R., Kersten, B., and Schnitzler, J. P. (2025). “Patterns of adaptation to drought in Quercus robur populations in central European temperate forests,” Global Change Biology 31, article e70168. https://doi.org/10.1111/gcb.70168

Olarescu, A., Cionca, M., and Gurau, L. (2016). “Physical and mechanical properties of wood from thin logs of Quercus petraea spp,” Environmental Engineering and Management Journal 15(12), 2695-2702. https://eemj.eu/index.php/EEMJ/article/view/3139

Olesen, P. O. (1971). “The water displacement method: A fast and accurate method of determining the green volume of wood samples,” Forest Tree Improvement 3, 1-23.

Ozyhar, T., Mohl, L., Hering, S., Hass, P., Zeindler, L., Ackermann, R., and Niemz, P. (2016). “Orthotropic hygric and mechanical material properties of oak wood,” Wood Material Science & Engineering 11(1), 36-45. https://doi.org/10.1080/17480272.2014.941930

Phipps, R. (1985). “Collecting, preparing, crossdating, and measuring tree increment cores: U.S. Geological Survey Water-Resources Investigations Report”, 85-4148. https://doi.org/10.3133/wri854148.

Pretzsch, H., Schütze, G., and Uhl, E. (2013). “Resistance of European tree species to drought stress in mixed versus pure forests: Evidence of stress release by inter-specific facilitation,” Plant Biology 15(3), 483-495. https://doi.org/10.1111/j.1438-8677.2012.00670.x

Provost, G. L., Brachi, B., Lesur, I., Lalanne, C., Labadie, K., Aury, M., Silva, C. D., Postolache, D., Leroy, T., and Plomion, C. (2022). “Gene expression and genetic divergence in oak species highlight adaptive genes to soil water constraints,” Plant Physiology 190(4), article 2466. https://doi.org/10.1093/plphys/kiac420

Radaković, N., and Stajić, B. (2021). “Climate signals in earlywood, latewood and tree-ring width chronologies of sessile oak (Quercus petraea (Matt.) Liebl.) from Majdanpek, North-Eastern Serbia,” Drvna Industrija 72(1), 79-87. https://doi.org/10.5552/drvind.2021.2016

Roibu, C., Sfeclă, V., Mursa, A., Ionita, M., Nagavciuc, V., Chiriloaei, F., Leșan, I., and Popa, I. (2020). “The climatic response of tree ring width components of ash (Fraxinus excelsior L.) and common oak (Quercus robur L.) from Eastern Europe,” Forests 11(5), article 600. https://doi.org/10.3390/f11050600

Romagnoli, M., Cavalli, D., and Spina, S. (2014). “Wood quality of chestnut: Relationship between ring width, specific gravity, and physical and mechanical properties,” BioResources 9(1), 1132-1147.

Römer, P., Wieland, A., Torbenson, M. C., Reinig, F., Ziaco, E., Frigo, D., Greule, M., Urban, O., Čáslavský, J., Pernicová, N., Trnka, M., Carrer, M., Büntgen, U., Keppler, F., and Esper, J. (2025). “Covariance and climate signals among state-of-the-art tree-ring proxies,” Quaternary Science Reviews 355, article 109270. https://doi.org/10.1016/j.quascirev.2025.109270

Roszyk, E., Moliński, W., and Jasińska, M. (2010). “The effect of microfibril angle on hygromechanic creep of wood under tensile stress along the grains,” Wood Research 55(3), 13-24.

Rybníček, M., Čermák, P., Žid, T., Kolář, T., Trnka, M., and Büntgen, U. (2015). “Exploring growth variability and crown vitality of sessile oak (Quercus Petraea) in the Czech Republic,” Geochronometria 42(1), 17-27. https://doi.org/10.1515/geochr-2015-0003

Schniewind, A. P. (1989). Concise Encyclopedia of Wood & Wood-Based Materials, Pergamon Press, Oxford, UK.

Schweingruber, F. H., Fritts, H. C., Braker, O. U., Drew, L. G., and Schär, E. (1978). “The X-ray densitometric method as applied to dendrochronology,” Tree-Ring Bulletin 38, 61-91.

Sejdiu, R., Hoxha, F., Jashari, B., and Idrizi, L. (2020). “Physical properties of sessile oak (Quercus petraea L) used by the wood industry in Kosovo,” Technium: Romanian Journal of Applied Sciences and Technology 2(7), 278-285. https://doi.org/10.47577/technium.v2i7.2009

Seidl, L., Keya, S., Seiwald, L., Hage, S., Huber, H., and Pakarinen, T. (2024). “Reusing salvaged wood in buildings: Non-destructive-testing methods for early-stage decision making,” Puuwood 1-12.

Sochová, I., Kolář, T., and Rybníček, M. (2021). “A review of oak dendrochronology in Eastern Europe,” Tree-Ring Research 77(1), 10-19. https://doi.org/10.3959/TRR2020-2

Souto-Herrero, M., Rozas, V., and García-González, I. (2018). “Chronologies of earlywood vessels and latewood width disentangle climate drivers of oak growth in a mild oceanic region,” Dendrochronologia 51, 40-53. https://doi.org/10.1016/j.dendro.2018.07.004

Spiecker, H., Mielikäinen, K., Köhl, M., and Skovsgaard, J. P. (1996). Growth Trends in European Forests: Studies from 12 Countries, European Forest Institute Research Report 5, Springer-Verlag, Berlin.

Špulák, O., Slodičák, M., Novák, J., and Leugner, J. (2024). “Postupy hospodaření v porostech dubu zimního pro zmírnění nepříznivých dopadů klimatické změny,” Lesnický průvodce (Management practices in sessile oak stands to mitigate adverse effects of environmental change), 5/2024. Forestry and Game Management Research Institute, Brno. ISBN 978-80-7417-278-6, ISSN 0862-7657.

Terrasse, F., Brancheriau, L., Marchal, R., Boutahar, N., Lotte, S., Guibal, D., Pignolet, L., and Candelier, K. (2021). “Density, extractives and decay resistance variabilities within branch wood from four agroforestry hardwood species,” iForest 14, 212-220. https://doi.org/10.3832/ifor3693-014

Torbenson, M., Büntgen, U., Römer, P., Urban, O., Trnka, M., Ač, A., Reinig, F., Rybníček, M., Kolář, T., Arosio, T., Martinez del Castillo, E., Koňasová, E., Pernicová, N., Čáslavský, J., and Esper, J. (2023). “Assessing earlywood-latewood proportion influence on tree-ring stable isotopes,” Dendrochronologia 82, article 126147. https://doi.org/10.1016/j.dendro.2023.126147

Triplat, M., and Krajnc, N. (2017). “A system for quality assessment of forestry contractors,” Croatian Journal of Forest Engineering 42(1), 14. https://doi.org/10.5552/crojfe.2021.834

Uldry, A., Husted, B.P., Pope, I., and Ottosen, L. M. (2024). “A review of the applicability of non-destructive testing for the determination of the fire performance of reused structural timber,” Journal of Nondestructive Evaluation 43, 106. https://doi.org/10.1007/s10921-024-01120-6

Vavrčík, H., and Gryc, V. (2012). “Analysis of the annual ring structure and wood density relations in English oak and Sessile oak,” Wood Research 57(4), 573-580.

Viewegh, J., Kusbach, A., and Mikeska, M. (2003). “Czech forest ecosystem classification,” Journal of Forest Science 49(2), 74-82.

Vitali, V., Martínez-Sancho, E., Treydte, K., Andreu-Hayles, L., Dorado-Liñán, I., Gutierrez, E., Helle, G., Leuenberger, M., Loader, N., Rinne-Garmston, K. T., Schleser, G. H., Allen, S., Waterhouse, J. S., Saurer, M., and Lehmann, M. M. (2022). “The unknown third Hydrogen isotopes in tree-ring cellulose across Europe,” Science of The Total Environment 813, article 152281. https://doi.org/10.1016/j.scitotenv.2021.152281

Walker, J. C. F. (ed.). (2006). Primary Wood Processing: Principles and Practice (2nd Ed.), Springer, Dordrecht. https://doi.org/10.1007/1-4020-4393-7

Wang, X. (2021). “Recent advances in nondestructive evaluation of wood: In-forest wood quality assessments,” Forests 12, article 949. https://doi.org/10.3390/f12070949

Wimmer, R. (2002). “Wood anatomical features in tree-rings as indicators of environmental change,” Dendrochronologia 20(1-2), 21-36. https://doi.org/10.1078/1125-7865-00005

Wu, D., Seibold, S., Pietsch, K. A., Ellwood, M. F., and Yu, M. (2023). “Tree species richness increases spatial variation but not overall wood decomposition,” Soil Biology and Biochemistry 183, article 109060. https://doi.org/10.1016/j.soilbio.2023.109060

Xie, W., Ding, Y., Wang, Z., Gao, Z., Zhang, T., Zhou, Y., He, Y., and Huang, X. (2020). “Testing and analysis of hemlock cross laminated timber,” Wood Research 65(5), 819-832. https://doi.org/10.37763/wr.1336-4561/65.5.819832

You, R., Zhu, N., Deng, X., Wang, J., and Liu, F. (2021). “Variation in wood physical properties and effects of climate for different geographic sources of Chinese fir in subtropical area of China,” Scientific Reports 11, article 4664. https://doi.org/10.1038/s41598-021-83500-w

Zhang, L., Han, Y., Xie, Q., Wang, Y., and Wu, Y. (2024). “Mechanical performance of wood subjected to the interaction of transversal tension/compression and longitudinal shear stresses,” Construction and Building Materials 420, article 135637. https://doi.org/10.1016/j.conbuildmat.2024.135637

Zhao, X., Wang, D., Guo, P., Feng, Q., and Deng, Y. (2025). “Accuracy of increment core method for measuring basic wood density and moisture content in three Catalpa species,” Plants 14(15), article 2339. https://doi.org/10.3390/plants14152339

Zobel, B. J., and Talbert, J. T. (1984). Applied Forest Tree Improvement, John Wiley & Sons, New York.

Article submitted: June 24, 2026; Peer review completed: July 25, 2026; Revised version received: September 10, 2026; Accepted: September 11, 2026; Published: November 1, 2026.