Abstract
New methods for the synthesis of metal-containing composite materials based on natural polymers (chitosan, organosolv lignin, and nanocellulose) are proposed. Metal doping was performed by introducing salts of Cu(CH3COO)2, Ni(NO3)2, and Co(NO3)2 into a suspension of the initial biopolymer mixture. The obtained chitosan–cellulose (C/C) and chitosan–lignin (C/L) composites have a sponge-like structure and they are predominantly macroporous (cavity size from 50 to 70 μm). Analysis revealed the formation of three-dimensional structures with relatively loose packing, with a surface morphology resembling foam. The thermal stability of C/L biocomposites decreased in sequence: C/L > C/L/Ni > C/L/Cu > C/L/Сo. Cobalt-containing carbon composites obtained by carbonization of C/L and C/C samples at 600°C exhibited high specific surface area and pore volume. These composites were micro/mesoporous materials with mesopore fractions of 76.5% and 64.7%, respectively. Carbonization of the nickel-containing C/C biocomposite at 600 °C yielded a carbon composite with a predominantly microporous structure. The influence of the introduced metal nature, organic matrix composition, and carbonization temperature on the morphology and microstructure of the carbon composites was studied by SEM, XRD, and spectral chemical analysis methods. Samples carbonized at 400 to 600 °C consisted of three-dimensional structures of randomly linked film fragments with large cells. The distribution of the metal (Co, Ni, Cu) over the carbon support surface was found to be uniform.
Download PDF
Full Article
Synthesis and Properties of Copper-, Nickel-, and Cobalt-Doped Carbonized Composites Based on Chitosan, Organosolv Lignin, and Nanocellulose
Nadezhda M. Mikova ,a,* Anatoly M. Zhyzhaev
,a Ivan P. Ivanov
,a Olga Yu Fetisova
,a Yaroslav I. Ageev
,a Oxana P. Taran
,a,b and Boris N. Kuznetsov
,a,b
New methods for the synthesis of metal-containing composite materials based on natural polymers (chitosan, organosolv lignin, and nanocellulose) are proposed. Metal doping was performed by introducing salts of Cu(CH3COO)2, Ni(NO3)2, and Co(NO3)2 into a suspension of the initial biopolymer mixture. The obtained chitosan–cellulose (C/C) and chitosan–lignin (C/L) composites have a sponge-like structure and they are predominantly macroporous (cavity size from 50 to 70 μm). Analysis revealed the formation of three-dimensional structures with relatively loose packing, with a surface morphology resembling foam. The thermal stability of C/L biocomposites decreased in sequence: C/L > C/L/Ni > C/L/Cu > C/L/Сo. Cobalt-containing carbon composites obtained by carbonization of C/L and C/C samples at 600°C exhibited high specific surface area and pore volume. These composites were micro/mesoporous materials with mesopore fractions of 76.5% and 64.7%, respectively. Carbonization of the nickel-containing C/C biocomposite at 600 °C yielded a carbon composite with a predominantly microporous structure. The influence of the introduced metal nature, organic matrix composition, and carbonization temperature on the morphology and microstructure of the carbon composites was studied by SEM, XRD, and spectral chemical analysis methods. Samples carbonized at 400 to 600 °C consisted of three-dimensional structures of randomly linked film fragments with large cells. The distribution of the metal (Co, Ni, Cu) over the carbon support surface was found to be uniform.
DOI: 10.15376/biores.21.4.12121-12138
Keywords: Biocomposites; Chitosan; Organosolv lignin; Nanocellulose; Metal doping; Carbonization; Carbon composites; Structure
Contact information: a: Institute of Chemistry and Chemical Technology SB RAS, FRC KSC SB RAS, Akademgorodok 50, bld., Krasnoyarsk 660036, Russia; b: Siberian Federal University, pr. Svobodny 79, Krasnoyarsk 660041, Russia; *Corresponding author: [email protected]
Graphical Abstract
INTRODUCTION
Currently, researchers are actively developing composite materials based on natural biopolymers such as chitosan, cellulose, lignin, and their derivatives (Zain et al. 2014; Kun and Pukánszky 2017; Bakshi et al. 2020; Syduzzaman et al. 2020). Interest in using these renewable polymers is driven by the increasing need to reduce global consumption of fossil resources. The most common methods for creating new composite biomaterials are based on using mixtures of different polymers. In the synthesis of biocomposites, additional components such as carbon particles (Dong et al. 2021), metal compounds (Zain et al. 2014; Căprărescu et al. 2020), and various polymers (Chen et al. 2009; Khalil et al. 2016; Zhu et al. 2019) are used. This technological approach, known as “green synthesis”, aims to produce environmentally friendly materials with improved characteristics or desired properties (Zain et al. 2014; Khalil et al. 2016).
Biocomposites based on chitosan and cellulose with silver (Căprărescu et al. 2020; Ahamed et al. 2015) and copper (Valodkar et al. 2011) additives are intended for use as bactericidal agents in medicine and antimicrobial therapy. Polymer composites are widely used in various adsorption processes, such as water purification from heavy metals and dyes, nanofiltration, etc. (Thakur and Voicu 2016; Căprărescu et al. 2020; Dong et al. 2021; Mikova et al. 2025).
In addition to applications in environmental protection or biomedicine, chitosan–polymer composites containing metal ions can be used to create new materials for sorption, catalysis, and electrical engineering (Guibal et al. 2014). For example, a composite material based on chitosan containing silver ions selectively adsorbs sulfur-containing pesticides (Yoshizuka et al. 2000), chitosan membranes containing copper nanoparticles effectively adsorb chromates and vanadates (de Godoi et al. 2013).
Carbonization of organic composites doped with metals allows the production of carbon composites containing metal nanoparticles in various oxidation states. The structural characteristics of the carbon composite and the state of the metal-containing particles can be altered by varying the pyrolysis temperature. The produced metal-doped carbon composites are attractive for the use as catalysts, catalyst supports, and adsorbents (Cotet et al. 2006; Raptopoulos et al. 2021; Abdullahi and Muhammad 2025). The morphology and structure of the carbon composite surface depend on the nature of the introduced metal. For example, among the carbon fiber composites based on alginate doped with Co, Ni, Cu, the cobalt-containing sample exhibited the highest degree of graphitization (Raptopoulos et al. 2021).
Carbon composites containing metal oxides (NiO, CoO, and MoO3) were effective catalysts for hydrodeoxygenation of biomass (Abdullahi and Muhammad 2025; Yan et al. 2025). Copper-containing carbon catalysts were used in the electrocatalytic hydrogenation of CO2 (Xiao et al. 2019). Carbon catalysts containing nickel oxide nanoparticles showed high catalytic activity in rice husk pyrolysis (Saravana Sathiya Prabhahar et al. 2024).
A new method for producing chitosan–cellulose materials in the form of composite sponges was proposed in a previously reported study (Mikova et al. 2026). Chitosan and a cellulose aerogel based on birch alpha-cellulose were used as components to create the chitosan–cellulose matrix. By carbonization of chitosan–cellulose biocomposites at 600 °C followed by thermo-alkaline activation with NaOH at 800 °C, carbon materials with a developed porous structure were obtained. The highest specific surface area (1160 m2/g) had the activated carbon composite modified with tannin. This sample contained a significant fraction of mesopores with sizes ranging from 2 to 17 nm. The activated copper-containing carbon composite had a lower specific surface area (588 m2/g) and predominantly microporous structure. These results demonstrate that the chemical composition of initial organic composite may affect the structure of the resulting carbon product.
In this study the new methods for synthesis of metal-containing carbon composite materials based on carbonization of natural polymers (chitosan, organosolv lignin and nanocellulose) modified by salts of Cu(CH3COO)2, Ni(NO3)2 and Co(NO3)2 were proposed.
The influence of the introduced metal nature, organic matrix composition and carbonization temperature on the morphology and microstructure of carbon composites was established.
EXPERIMENTAL
For synthesis of the biocomposite, chitosan, pine organosolv lignin, and nanocellulose were used. Chitosan sample was obtained from ZAO “Bioprogress” (TU 9289-067-00472124-03); it had an average molecular weight of 260 kDa. The elemental composition of the chitosan (wt%) was C – 41.41%; H – 6.69%; N – 7.05%; and O – 44.85%.
Organosolv lignin was isolated from pinewood. The sawdust was first crushed to a fraction of 0.5 to 1.0 mm followed by treatment with a 60% aqueous ethanol solution in an autoclave at 180 °C according to the reported procedure (Weinwurm et al. 2014). The elemental composition of the organosolv lignin was (wt%): C – 70.7%; H – 6.7%; and O – 22.6%.
Regenerated nanocellulose was obtained in the form of cellulose aerogel from a solution of pine wood alpha-cellulose in 9% NaOH following the procedure of Kuznetsov et al. (2022). The preparation method included successive steps of dissolution, freeze–drying, precipitation, and washing. Chemical composition of nanocellulose (wt%): cellulose 96.0%; lignin 1.1%; and hemicellulose 2.9%. Elemental composition of nanocellulose (wt%): C – 42.6%; H – 6.30%; and O – 51.1%.
Organic biocomposites were prepared by mixing a 2% chitosan (C) solution with cellulose (Cel) or lignin (L) in mass ratios of 5:1 and 2:1. The salts (Cu(CH3COO)2, Ni(NO3)2, and Co(NO3)2) were then added to the suspension in a mass ratio of 0.5:10 with respect to the organic polymers. The suspension components were stirred for 1.0 h at 50 °C. After cooling to 25 °C, the mixture was placed in a refrigerator, held for 12 h at –18 °C, and then freeze-dried using the Iney-6 apparatus (Moscow, Russia). The samples were labeled using designations for the initial polymer components and the introduced metal salts: C/L/Cu, C/Cel/Cu, C/L/Ni, C/Cel/Ni, C/L/Co, and C/Cel/Co.
For the preparation of carbon composites, the biocomposite samples were placed in corundum crucibles and carbonized in a tubular electric furnace in argon atmosphere. The heating rate was 10 °C/min, and the holding time at the final temperature (400 to 800 °C) was 1 h. Carbonized samples are labeled using designations for the initial polymer components, metal additives, and the pyrolysis temperature (400, 600, or 800 °C); for example: C/L/Cu-400, C/Cel/Cu-400, C/L/Ni-600, C/L/Co-600, etc.
The elemental composition of the composite samples was determined using a Vario EL Cube CHN analyzer (Germany). The oxygen content was calculated by difference.
Infra-red (IR) absorption spectra of the samples in the range of 4000 to 500 cm-1 were recorded using an IR Tracer-100 FTIR spectrometer (Shimadzu, Japan). Initial samples were prepared as pellets by mixing with KBr at a mass ratio of substance/matrix at 3.0 mg/1000 mg, followed by pressing. Spectra were recorded at a resolution of 4 cm-1 using 32 scans. Spectral information was processed using LabSolution IR software.
The textural characteristics of the prepared composites were calculated from the nitrogen adsorption–desorption isotherms measured at –196 °C at a relative pressure (P/Po) of 0.005 to 0.995 using an ASAP 2020 automatic adsorption analyzer (Micromeritics, USA). Before starting the measurement, the samples were degassed at 200 °C for 12 h under vacuum. The pore structure of the samples was characterized by the following parameters: the specific surface area, determined by the Brunauer-Emmett-Teller method (SBET) using the adsorption isotherm, and the total pore volume (Vtotal) was calculated from the volume of nitrogen adsorbed at P/P0 ≥ 0.995. The mesopore size distribution was calculated by the Barrett-Joyner-Halenda (BJH) method using the software supplied with the ASAP 2020 automatic adsorption apparatus. The micropore volume was calculated using the t-method, and the micropore size was determined via the DFT method.
The morphology of the samples was examined by scanning electron microscopy (SEM) in backscattered electron imaging mode with the use of a TM-4000 device (Hitachi, Japan) with integrated energy dispersion spectrometer Bruker and in secondary electron imaging mode (S5500 device with accelerating voltage of 20 kV, resolution of 20 microns).
The XRD study was carried out using DRON-3M (S-Petersburg, Russia) X-ray diffractometer (CuKα monochromatized radiation with λ = 1.5406 Å). The measurements were performed in within the Bragg angle range 2θ 5° – 70 ° at the scan step with 0.01 % scan. The accumulation time at the point was 1 second.
Thermogravimetric analysis was achieved using STA 449F1 Jupiter analyzer (Netzsch, Germany). The sample was heated from 30 to 800 °C at a rate of 10 °C/min in a corundum crucible in an argon atmosphere. The measurement results were processed using the NETZSCH Proteus Thermal Analysis 5.1 software package.
RESULTS AND DISCUSSION
Characteristics of Organic Biocomposites
After freeze-drying, the organic biocomposite samples were obtained as thin-walled foam (sponge) covered on the outer surface with a transparent mesh film.
The elemental analysis (Table 1) revealed that chitosan–lignin composites contain more carbon than chitosan–cellulose samples. Their average density ranged from 0.044 to 0.059 g/cm3, while the density of chitosan–cellulose samples were between 0.041 and 0.043 g/cm3.
Table 1. Elemental Composition and Density of Biocomposite Samples
Infrared spectroscopy
Fourier transform infra-red (FTIR) spectra of organosolv lignin, chitosan, and the obtained composites (chitosan–cellulose and chitosan–lignin) were compared (Fig. 1). The spectrum of lignin (Fig. 1-1) reflects its complex structure, containing various functional groups such as hydroxyl, phenolic, carboxyl, methoxyl, aldehyde, alkyl– and aryl–ether groups, etc. (Derkacheva et al. 2018). The spectrum of chitosan (Fig. 1-2) shows considerable similarity to that of cellulose (Thakur and Voicu 2016; Zhang et al. 2020; Mikova et al. 2026), indicating good molecular compatibility between chitosan and cellulose (Vega-Cázarez et al. 2018). In the frequency range of 3500 to 3300 cm-1, characteristic absorption bands for chitosan were observed, which corresponded to the stretching vibrations of hydroxyl groups, as well as symmetric and asymmetric vibrations of N–H in amino groups (Lv et al. 2014).
Fig. 1. IR spectra of lignin (1), chitosan (2), chitosan–lignin composite (3), and chitosan–cellulose composite (4) samples
The IR spectra of chitosan-lignin (C/L) and chitosan-cellulose (C/Cel) composites were similar. The overlap of νO–H stretching vibrations of cellulose and phenolic OH groups of lignin with νN–H stretching vibrations of the amino group (–NH2) led to a shift and significant broadening of the bands, indicating the formation of hydrogen bonds between these functional groups (Duan et al. 2015; Vega-Cázarez et al. 2018).
The difference between the IR spectra of the C/L and C/Cel samples was revealed by the peaks at 1513 and 1267 cm-1, which indicate the presence of guaiacyl aromatic structures (G-type) characteristic of the initial organosolv lignin (Mikova et al. 2018). The phenolic OH groups of lignin, capable of forming hydrogen bonds, interact with hydroxyl groups and amino groups of chitosan (Kun and Pukánszky 2017; Rosova et al. 2021; Ji et al. 2022). The results from IR spectroscopy indicate that the intermolecular hydrogen bonds play a key role in the formation of C/L and C/Cel biocomposites.
SEM and XRD analyses
SEM method was used for the study of morphological features of chitosan–polymer composites. The C/L and C/Cel biocomposite samples have three-dimensional structures randomly formed from flat non-porous fragments (Fig. 2). The formed cavities and macropores in biocomposites have sizes up to several tens of microns.
Fig. 2. SEM images of chitosan–cellulose (A); and chitosan–lignin (B) biocomposite samples
The copper-containing C/L composite has a three-dimensional microstructure with loose packing, resembling foam in surface morphology (Fig. 3A). The three-dimensional structures of C/L composites doped with Ni and Co show less pronounced relief of surface (Fig. 3B, 3C).
Fig. 3. SEM images of metal-doped chitosan–lignin biocomposites: C/L/Cu (А), C/L/Ni (B), and C/L/Co (С)
In the SEM images of these samples, closed cells are extremely rare; only individual cavities with smooth walls are present.
XRD results showed that copper, nickel, and cobalt do not form separate phases on the surface of the metal-doped biocomposites.
Thermogravimetric study
The thermochemical properties of C/L composites were studied by thermo-gravimetric analysis (TGA). The TGA and DTG curves for these samples are shown in Fig. 4, and some characteristics of their thermal degradation are presented in Table 2.
Thermal decomposition of lignin samples began above 200 °C and proceeded with high intensity in the temperature range of 222 to 459 °C (Table 2). On the DTG curve, this interval was characterized by an intense peak at 393 °C and a less pronounced shoulder at about 240 °C (Fig. 4B). In this temperature range, depolymerization processes such as cleavage of C–C bonds inside chains, destruction of ether bonds etc., occur. This is accompanied by the removal of low-molecular-weight fragments (Kawamoto 2017; Raptopoulos et al. 2021).
Fig. 4. Thermograms of chitosan–lignin biocomposites: TGA (A); and DTG (B)
Table 2. Some Characteristics of the Thermal Degradation of Lignin and Chitosan–Lignin Samples
With a further increase in temperature (above 450 °C), the mass loss rate of lignin decreased significantly, and the thermodegradation process continued up to 800 °C. At this stage, deep aromatization of the lignin sample occurred with the formation of a carbon residue at 36.9% to 42.1% (wt% basis). The significant yield of carbon residue could be attributed to the high thermal stability of the aromatic components of lignin (Missio et al. 2018).
The onset of thermal degradation of C/L biocomposites occurred at lower temperatures than that of lignin samples, due to the weakening of intra- and intermolecular hydrogen bonds in the composite (Cai et al. 2018). Analysis of the TG/DTG curves of C/L composites containing Ni, Cu, and Co revealed three pyrolysis regions: the first below 250 °C, the second between 250 and ~400 °C, and the third above 400 °C. The similar decomposition stages for alginate- and polyurea-based biocomposites containing Co, Ni, and Cu were observed by Raptopoulos et al. (2021).
In the range below 250 °C, the samples still contain free water, which causes weight loss at temperatures up to 200 °C. Mass loss in this temperature range can also be caused by the removal of low-molecular-weight compounds adsorbed on the sample surface. The first mass loss of the samples is 11.2% for C/L/Co, 12% for C/L/Cu, and 16.5% for C/L/Ni.
The second temperature range (200 to 400 °C), where the main mass loss occurred, is associated with intense thermal degradation of the polymer chains of both chitosan and lignin. The mass loss of samples in this interval is 29.8% for C/L/Co, 30.1% for C/L/Ni, and 32.5% for C/L/Cu.
The third pyrolysis region is associated with aromatization processes leading to the formation of a carbon residue in the temperature range from 341 to 366 °C to 800 °C.
The thermal behavior of the studied C/L composites with introduced metal ions (Ni, Cu, Co) also exhibit similar thermal destruction behavior. Metal salts can weaken the hydrogen bonds between chitosan and lignin, which contributes to a decrease in the temperature of thermodegradation of the biocomposite (Voronova et al. 2020). At the same time, the nature of the introduced metal influences the temperature of maximum mass loss, the yield of solid residue, and the rate of thermodegradation (Table 2). If the temperature of the maximum mass loss rate is taken as a characteristic of thermal stability, the samples of lignin and biocomposites are arranged in the following order, as their thermal stability decreases: L > C/L > C/L/Ni > C/L/Cu > C/L/Сo
During the thermal transformation of C/L composites containing metals, along with carbonization of the organic matrix, a change in the state of the metal-containing compounds incorporated into the composite structure occurred. The mechanism of thermal transformation of such systems is complex and depends on the nature of the organic matrix and the metal, the state of the metal and its degree of dispersion, as well as the nature of the interaction of the metal with the polymer matrix (Căprărescu et al. 2020).
CHARACTERISTICS OF CARBON COMPOSITES
Study of Textural Characteristics by BET Method
Specific surface area (SBET), external surface area (Sext), total pore volume (Vpore), micropore surface area and volume (Smicro, Vmicro), average pore diameter (Dpore), and average mesopore size (DBJH) of carbon composites are given in Table 3.
The porous structure of the carbon composites was largely determined by the carbonization temperature of the initial biocomposite. With increasing carbonization temperatures from 400 to 600 °C, the specific surface area of C/L samples increased from 6 to 12 m2/g, that of C/Cel/Cu from 8 to 25 m2/g, and that of C/L/Ni from 37 to 207 m2/g, respectively.
The porous characteristics of metal-containing carbon composites also depended on the nature of metal and polymeric matrix. The influence of these parameters can be traced using the carbonization of cobalt-modified C/Cel and C/L biocomposites as examples. The carbon composite obtained by carbonization at 600 °C of Co-containing chitosan–lignin composite (C/L/Co-600) had the most developed porosity. Its specific surface area was 446 m2/g, total pore volume was 0.515 cm3/g, and the mesopore volume fraction was 76.5%.
The carbon composite on the basis of Co-containing chitosan–cellulose biocomposite (C/Cel/Co-600) was less porous. Its specific surface area was 316 m2/g, total pore volume was 0.190 cm3/g, and the mesopore fraction was 70.5%. The decrease in the volume of micropores occurred simultaneously with an increase in the volume of meso- and macro-pores in the sample.
Table 3. Textural Characteristics of Carbon Composites
The carbon composite obtained by carbonization at 800 °C of the chitosan–lignin–cellulose biocomposite (C/L/Cel-800) had a specific surface area of 423 m2/g, a total pore volume of 0.172 cm3/g, and the smallest micropore diameter of 1.63 nm. The micropore volume fraction was 70.35%.
The shape of the nitrogen adsorption–desorption isotherms indicate their microporous/mesoporous structure on the carbon composite samples (Fig. 5) (Gregg and Sing 1991).
Fig. 5. Nitrogen absorption–desorption isotherms: 1: Carbon sample C/L/Ni-600; 2: Carbon sample C/Cel/L-800; 3: Carbon sample C/Cel/Co-600; 4: Carbon sample C/L/Co-600
Figure 6 demonstrates the pore size distribution in carbon composite samples obtained at 600 °C. The carbon samples C/L/Co-600 contains narrow micropores with a size < 2 nm (Fig. 6A-1). According to the BJH method, this sample had the largest volume of mesopores with a size of 2 to 12 nm (Fig. 6B-1).
Fig. 6. Dependence of meso- and micropore volume distribution, calculated by the DFT method (A) and by the BJH method (B), on pore size in carbon composites: 1 – C/L/Co-600; 2 – C/L/Ni-600; 3 – C/Cel/Co-600
The carbon composite C/Cel/Co-600 had a large volume of micropores of sizes less < 2 nm (Fig. 6A-3). Micropores of size 1.5 to 2.0 nm were dominant in carbon composite C/L/Ni along with small amount of mesopores of sizes less 12 nm (Fig. 6B-2).
Study of morphology and structure by SEM and XRD methods
In the SEM images of carbon composite carbonized at 400 °C, three-dimensional structures of randomly linked film fragments with large cells (up to 50 μm and more) are present (Fig. 7). The carbon composite C/Cel/L-400 contains nanocellulose fragments (marked with a circle) in its structure (Fig. 7B). The structure of the copper-containing carbon composite C/Cel/Cu-400 is characterized by extended and layered film fragments with a smooth surface (Fig. 7C).
Fig. 7. SEM images of carbon composites carbonized at 400 °C: A – C/L-400; B – C/Cel/L-400; C – C/Cel/Cu-400
After carbonization of metal-containing biocomposites at 400 °C, the distribution of Co, Ni, and Cu metals on the carbon surface remained uniform.
Increasing the carbonization temperature from 400 °C to 600 °C increased the porosity of carbon composites. The porosity of the carbon sample C/Cel-600 was mainly determined by carbon fibers formed from cellulose (Fig. 8A). The carbon composite C/L-600 had a grooved surface with numerous depressions and folds (Fig. 8B). After carbonization at 600 °C, a significant transformation of the morphology of the Cu-containing C/L carbon composite was observed (Fig. 8C). The porous structure of this sample contained channels, cavities, and voids, the sizes of which reach several microns.
Fig. 8. SEM images of carbon composites: C/Cel-600 (A), C/L-600 (B), C/L/Cu-600 (C)
As a result of carbonization, the carbon and metal contents increased in the composites doped with copper, nickel, and cobalt. In the carbon composite C/L/Cu-600, the copper content was about 20 wt%, and the metal distribution in the carbon matrix was uniform. The absence of copper particles on the surface of carbon black impregnated with a copper–ammonia complex and heated at 500 °C is explained by the fact that copper was localized on nitrogen atoms incorporated into the carbon matrix (Xie et al. 2018).
After carbonization at 600 °C the sample C/L/Cu acquired a reddish tint, probably due to the presence of metallic copper particles. A similar phenomenon was observed during the thermal decomposition of CuSO4 supported on carbon nanotubes, which was explained by the carbothermal reduction of copper ions to metallic particles (Charnvanichborikarn et al. 2014). The results of elemental mapping of the carbon sample C/L/Ni-600 indicate a uniform distribution of nickel. According to X-ray fluorescence analysis, the nickel content in the sample was about 7 wt%, which was lower compared to samples containing Cu (20 wt%). The reduced nickel content may be due to removal from the sample as nickel carbonyl during high-temperature treatment.
Fig. 9. Diffractograms of carbon composites C/L/Co-600 (1) and C/L/Ni-600 (2).
Identified phase symbols: ● – metallic cobalt, ■ – metallic nickel
On the diffractograms of carbon samples C/L/Co-600 and C/L/Ni-600 weak lines of metallic cobalt (Сo0, d = 2,06; 1,927; 1,77 Å, JCPDS, 15-806) (Fig. 9, line 1) and nickel (Ni0, d = 2,5; 2,15; 2,03 Å, JCPDS, 45-1027) (Fig. 9, line 2) are present indicating carbothermal reduction of Co2+ and Ni2+ ions at this temperature.
Elemental mapping results indicated a uniform distribution of cobalt in the C/L/Co-600 carbon composite (Fig. 10). The cobalt content in this sample was 12.1 wt%.
Thus, all metals (Cu, Ni, and Co) were uniformly distributed both in the organic biocomposites and after their carbonization at 400 and 600°C. Obviously, during the formation of the biocomposite samples, free–N–H groups of chitosan, –OH groups of cellulose, and phenolic OH groups of lignin interacted with metal ions, promoting their incorporation into the structure of the organic matrix. Subsequent pyrolysis at 400 °C or 600 °C provided the uniform localization of metal particles in the carbon matrix.
Fig. 10. SEM image of carbon composite C/L/Co-600 (A); distribution of Co on carbon surface (B); and histogram of element composition Co content in the carbon matrix (C)
Increasing the carbonization temperature of metal-containing biocomposites up to 800 °C led to a significant change in the morphology of the carbon surface and in the state of the introduced metal. The copper metal particles uniformly distributed in the carbon sample C/L/Cu-600 transform after heating this sample at 800 °C into copper crystallites (Fig. 11A).
Fig. 11. SEM images of carbon sample C/L/Cu-800 in backscattered (A) and secondary (B) electrons
Upon enlarging the image, it can be seen that particles on the carbon surface were small copper crystals of sizes 100 to 200 nm with an octahedral or icosahedral shape, that possibly had formed from nanocrystals of size 10 nm or less (Fig. 11B).
On diffractograms of carbon composites doped with Ni, Co, Cu and carbonized at 800 °C, distinct metal peaks were present, and no oxide compounds were observed (Fig. 12).
Fig.12. Diffractograms of carbon composites C/L/Ni-800 (1), C/L/Co-800 (2), and C/L/Cu-800 (3) with designation of identified phases. Symbols: ● – metallic cobalt (Сo0), ■ – metallic nickel (Ni0), ▼ – metallic copper (Cu0), ⯁ – graphite (C), 🞚 – crystalline carbon of the cliftonite type (C)
At a carbonization temperature of 800 °C the introduced metal was able to promote graphitization of the carbon matrix. The most intense and broad halo with a maximum in the Bragg angle of 17° to 25°, characterizing the amorphous carbon phase, was present on the diffractogram of carbon composite C/Cel/Ni-800 (Fig. 12, line 1).
On the diffractogram of the C/L/Co-800 sample, weak reflections were present that correspond to the graphite phase and the crystallized carbon phase of the cliftonite type (Fig. 12, line 2). The carbon matrices of carbon composite C/L/Co-800 had a higher degree of graphitization compared to composites containing nickel and copper. It was reported in (Raptopoulos et al. 2021) that among the three metals studied (Co, Ni, Cu) in alginate-based metal-containing carbon composites, cobalt contributed the highest degree of graphitization of the carbon matrix after heat treatment at 800 °C.
Thus, the interaction of ions Cu2+, Ni2+, Co2+ with N-H and O-H, groups of the chitosan, lignin, and cellulose promote their incorporation into organic matrix, and subsequent high-temperature carbonization leads to carbothermal reduction of ions to form metallic particles uniformly distributed in the composite carbon. The obtained porous carbon composites doped with Ni, Co, Cu particles have prospects for use as catalysts, catalyst supports, and adsorbents.
CONCLUSIONS
- New methods for producing Cu, Ni, and Co-containing organic and carbon composites based on chitosan, pine organosolv lignin, and pine nanocellulose were proposed.
- According to Fourier transform infrared (FTIR) data, the organic matrix was constructed by the formation of hydrogen bonds between amino and hydroxyl groups of polymeric components. The scanning electron microscope (SEM) method established the formation of biocomposites with three-dimensional microstructure and relatively loose packing, resembling foam in surface morphology. The sizes of pores formed by interconnected film fragments reached to several tens of micrometers. The chelating and complexing properties of chitosan allow effective retention of metal ions by both chitosan–lignin and chitosan–cellulose matrices.
- Metal-containing porous carbon composites were obtained by carbonization at 400 to 800 °C of chitosan–polymer composites doped by Cu(CH3COO)2, Ni(NO3)2, and Co(NO3)2. Their porous characteristics were defined with the use of BET method. It was shown that the porous structure of carbon composites were determined by the nature of the initial biocomposite and modifying metal as well as carbonization temperature. The increase of carbonization temperature from 400 °C to 600 °C increased the porosity of carbon composites. The carbon composite obtained by carbonization at 600 °C of Co-containing C/L and C/Cel biocomposites had the most developed porosity. Their specific surface area was 446 m2/g and 316 m2/g, total pore volume 0.515 cm3/g and 0.190 cm3/g, and mesopore fraction 76.5% and 70.5%, respectively.
- According to SEM data, carbon composites obtained at 400 to 600 °C had three-dimensional structures consisting of randomly linked film fragments with large cells (up to 50 microns and more). The distribution of the metal (Co, Ni, Cu) on the surface of the carbon composites was uniform. Weak lines of metallic cobalt and nickel were recorded on diffractograms of C/L composites containing Co and Ni after their carbonization at 600 °C. On the diffractogram of the copper-doped C/Cel composite, distinct peaks of metallic copper appear after carbonization at 800 °C.
ACKNOWLEDGEMENT
This study was funded by the Russian Science Foundation № 25-13-20007 (https://rscf.ru/project/25-13-20007/), grant from the Krasnoyarsk Regional Science Foundation. The facilities of the Krasnoyarsk Regional Center of Research Equipment of Federal Research Center “Krasnoyarsk Science Center, Siberian Branch of the Russian Academy of Sciences ” (FRC KSC SB RAS) were employed in this study.
REFERENCES CITED
Abdullahi, B. H., and Muhammad, A. U. (2025). “Activated carbon-supported catalysts for oil-to-hydrocarbon conversion: a review,” Academia Green Energy 2(4), article 7962. https://doi.org/10.20935/AcadEnergy7962
Ahamed, M. I. N., Sankar, S., Kashif, P. M., Basha, S. K. H., and Sastry, T. P. (2015). “Evaluation of biomaterial containing regenerated cellulose and chitosan incorporated with silver nanoparticles,” International Journal of Biological Macromolecules 72, 680-686. https://doi.org/10.1016/j.ijbiomac.2014.08.055
Bakshi, P. S., Selvakumar, D., Kadirvelu, K., and Kumar, N. S. (2020). “Chitosan as an environment friendly biomaterial – A review on recent modifications and applications,” International Journal of Biological Macromolecules 150, 1072-1083. https://doi.org/10.1016/j.ijbiomac.2019.10.113
Cai, B., Zhong, T., Chen, P., Fu, J., Jin, Y., Liu, Y., Huang, R., and Tan, L. (2018). “Preparation, characterization and in vitro release study of drug-loaded sodium carboxy-methylcellulose/chitosan composite sponge,” Plos One 13(10), article e0206275. https://doi.org/10.1371/journal.pone.0206275
Căprărescu, S., Zgârian, R. G., Tihan, G. T., Purcar, V., Eftimie Totu, E., Modrogan, C., Chiriac, A.-L., and Nicolae, C. A. (2020). “Biopolymeric membrane enriched with chitosan and silver for metallic ions removal,” Polymers 12(8), article 1792. https://doi.org/10.3390/polym12081792
Charnvanichborikarn, S., Shin, S. J., Worsley, M. A., Tran, I. C., Willey, T. M., van Buuren, T., Felter, T. E., Colvin, J. D., and Kucheyev, S. O. (2014). “Nanoporous Cu–C composites based on carbon-nanotube aerogels,” Journal of Materials Chemistry A 2(4), 962-967. https://doi.org/10.1039/C3TA14303A
Chen, L., Tang, C.-y., Ning, N.-y., Wang, C.-y., Fu, Q., and Zhang, Q. (2009). “Preparation and properties of chitosan/lignin composite films,” Chinese Journal of Polymer Science 27(05), 739-746. https://doi.org/10.1142/S025676790900444 8
Cotet, L. C., Gich, M., Roig, A., Popescu, I. C., Cosoveanu, V., Molins, E., and Danciu, V. (2006). “Synthesis and structural characteristics of carbon aerogels with a high content of Fe, Co, Ni, Cu, and Pd,” Journal of Non-Crystalline Solids 352(26), 2772-2777. https://doi.org/10.1016/j.jnoncrysol.2006.03.039
de Godoi, F. C., Rodriguez-Castellon, E., Guibal, E., and Beppu, M. M. (2013). “An XPS study of chromate and vanadate sorption mechanism by chitosan membrane containing copper nanoparticles,” Chemical Engineering Journal 234, 423-429. https://doi.org/10.1016/j.cej.2013.09.006
Derkacheva, O., Ishankhodzhaeva, M., and Fedorov, A. (2018). “Experimental and theoretical study of IR spectra of lignins,” Vestnik of Saint Petersburg University. Physics. Chemistry 5(63), 78-85. https://doi.org/10.21638/11701/spbu04.2018.201
Dong, Y.-D., Zhang, H., Zhong, G.-J., Yao, G., and Lai, B. (2021). “Cellulose/carbon composites and their applications in water treatment – A review,” Chemical Engineering Journal 405, article 126980. https://doi.org/10.1016/j.cej.2020.126980
Duan, J., Han, C., Liu, L., Jiang, J., Li, J., Li, Y., and Guan, C. (2015). “Binding cellulose and chitosan via intermolecular inclusion interaction: Synthesis and characterisation of gel,” Journal of Spectroscopy 2015, 1-6. https://doi.org/10.1155/2015/179258
Gregg, S. J., and Sing, K. S. W. (1991). Adsorption, Surface Area, and Porosity, Academic Press. https://books.google.ru/books?id=YhNRAAAAMAAJ
Guibal, E., Vincent, T., and Navarro, R. (2014). “Metal ion biosorption on chitosan for the synthesis of advanced materials,” Journal of Materials Science 49(16), 5505-5518. https://doi.org/10.1007/s10853-014-8301-5
Ji, M., Li, J., Li, F., Wang, X., Man, J., Li, J., Zhang, C., and Peng, S. (2022). “A biodegradable chitosan-based composite film reinforced by ramie fibre and lignin for food packaging,” Carbohydrate Polymers 281, article 119078. https://doi.org/10.1016/j.carbpol.2021.119078
Kawamoto, H. (2017). “Lignin pyrolysis reactions,” Journal of Wood Science 63(2), 117-132. https://doi.org/10.1007/s10086-016-1606-z
Khalil, H. P. S. A., Saurabh, C. K., Adnan, A. S, Nurul Fazita, M. R., Syakir, M. I., Davoudpour, Y., Rafatullah, M., Abdullah, C. K., Haafiz, M. K. M., and Dungani, R. (2016). “A review on chitosan-cellulose blends and nanocellulose reinforced chitosan biocomposites: Properties and their applications,” Carbohydrate Polymers 150, 216-226. https://doi.org/10.1016/j.carbpol.2016.05.028
Kun, D., and Pukánszky, B. (2017). “Polymer/lignin blends: Interactions, properties, applications,” European Polymer Journal 93, 618-641. https://doi.org/10.1016/j.eurpolymj.2017.04.035
Kuznetsov, B. N., Vasilyeva, N. Yu., Mikova, N. M., and Zhizhaev, A. M. (2022). “Synthesis and sulfation with sulfamic acid of aerogels based on birch-wood and cotton celluloses,” Journal of the Siberian Federal University. Chemistry 15(1), 57-68. https://doi.org/10.17516/1998-2836-0271
Lv, F., Wang, C., Zhu, P., and Zhang, C. (2014). “Characterization of chitosan microparticles reinforced cellulose biocomposite sponges regenerated from ionic liquid,” Cellulose 21(6), 4405-4418. https://doi.org/10.1007/s10570-014-0440-y
Mikova, N. M., Fetisova, O. Y., Pavlenko, N., and Chesnokov, N. V. (2018). “Study of thermal behavior of organosolv lignins isolated from fir and aspen wood,” Chemistry for Sustainable Development 26(4), 411-418. https://doi.org/10.15372/KhUR20180408
Mikova, N. M., Zhizhaev, A. M., Ivanov, I. P., and Kuznetsov, B. N. (2025). “Synthesis and properties of porous carbon-carbon composite materials based on larch bark biochars and spruce wood cellulose,” Russian Journal of Applied Chemistry 98(2), 136-146. https://doi.org/10.31857/s0044461825020067
Mikova, N. M., Zhizhaev, A. M., Ivanov, I. P., Fetisova, O. Yu., Ovchinnikova, T. G., and Kuznetsov, B. N. (2026). “Synthesis and properties of porous organic and carbon composites based on cellulose aerogel and chitosan,” Journal of Siberian Federal University. Chemistry 19(1), 37-50.
Missio, A. L., Mattos, B. D., Ferreira, D. d. F., Magalhães, W. L. E., Bertuol, D. A., Gatto, D. A., Petutschnigg, A., and Tondi, G. (2018). “Nanocellulose-tannin films: From trees to sustainable active packaging,”Journal of Cleaner Production 184, 143-151. https://doi.org/10.1016/j.jclepro.2018.02.205
Raptopoulos, G., Papastergiou, M., Chriti, D., Effraimopoulou, E., Čendak, T., Samartzis, N., Mali, G., Ioannides, T., Gurikov, P., and Smirnova, I. (2021). “Metal-doped carbons from polyurea-crosslinked alginate aerogel beads,” Materials Advances 2(8), 2684-2699. https://doi.org/10.1039/d0ma01025a
Rosova, E., Smirnova, N., Dresvyanina, E., Smirnova, V., Vlasova, E., Ivan’kova, E., Sokolova, M., Maslennikova, T., Malafeev, K., Kolbe, K., Kanerva, M., and Yudin, V. (2021). “Biocomposite materials based on chitosan and lignin: Preparation and characterization,” Cosmetics 8(1), article 24. https://doi.org/10.3390/cosmetics8010024
Saravana Sathiya Prabhahar, R., Jeyasubramanian, K., Nagaraj, P., and Sakthivel, A. (2024). “Catalytic pyrolysis of rice husk with nickel oxide nano particles: Kinetic studies, pyrolytic products characterization and application in composite plates,” Biomass Conversion and Biorefinery 14(2), 2849-2866. https://doi.org/10.1007/s13399-022-02703-x
Syduzzaman, M., Al Faruque, M. A., Bilisik, K., and Naebe, M. (2020). “Plant-based natural fibre reinforced composites: A review on fabrication, properties and applications,” Coatings 10(10), article 973. https://doi.org/10.3390/coatings10100973
Thakur, V. K., and Voicu, S. I. (2016). “Recent advances in cellulose and chitosan based membranes for water purification: A concise review,” Carbohydrate Polymers 146, 148-165. https://doi.org/10.1016/j.carbpol.2016.03.030
Valodkar, M., Modi, S., Pal, A., and Thakore, S. (2011). “Synthesis and anti-bacterial activity of Cu, Ag and Cu–Ag alloy nanoparticles: A green approach,” Materials Research Bulletin 46(3), 384-389. https://doi.org/10.1016/j.materresbull.2010.12.001
Vega-Cázarez, C. A., López-Cervantes, J., Sánchez-Machado, D. I., Madera-Santana, T. J., Soto-Cota, A., and Ramírez-Wong, B. (2018). “Preparation and properties of chitosan–PVA fibers produced by wet spinning,” Journal of Polymers and the Environment 26(3), 946-958. https://doi.org/10.1007/s10924-017-1003-8
Voronova, M. I., Surov, O. V., Afineevskii, A. V., and Zakharov, A. G. (2020). “Properties of polyacrylamide composites reinforced by cellulose nanocrystals,” Heliyon 6(11), article e05529. https://doi.org/10.1016/j.heliyon.2020.e05529
Weinwurm, F., Drljo, A., Silva, T. L., and Friedl, A. (2014). “Principles of ethanol organosolv lignin precipitation: Process simulation and energy demand,” Italian Association of Chemical Engineering. https://doi.org/10.3303/CET1439098
Xiao, X., Xu, Y., Lv, X., Xie, J., Liu, J., and Yu, C. (2019). “Electrochemical CO2 reduction on copper nanoparticles-dispersed carbon aerogels,” Journal of Colloid and Interface Science 545, 1-7. https://doi.org/10.1016/j.jcis.2019.03.005
Xie, X., Liu, J., Li, T., Song, Y., and Wang, F. (2018). “Post-formation copper-nitrogen species on carbon black: Their chemical structures and active sites for oxygen reduction reaction,” Chemistry – A European Journal 24(39), 9968-9975. https://doi.org/10.1002/chem.201801764
Yan, P., Peng, H., Rabiee, H., Ge, L., Weng, Y., Ma, B., Wang, J., Konarova, M., Zhao, G., Kennedy, E. M., Zhu, Z., and Stockenhuber, M. (2025). “Advances in lignocellulosic biomass pyrolysis and catalytic upgrading for sustainable biofuel production: process design strategies and reaction rationales,” Green Chemistry 27(35), 10444-10477. https://doi.org/10.1039/D5GC02199E
Yoshizuka, K., Lou, Z., and Inoue, K. (2000). “Silver-complexed chitosan microparticles for pesticide removal,” Reactive and Functional Polymers 44(1), 47-54. https://doi.org/10.1016/S1381-5148(99)00076-0
Zain, N. M., Stapley, A. G. F., and Shama, G. (2014). “Green synthesis of silver and copper nanoparticles using ascorbic acid and chitosan for antimicrobial applications,” Carbohydrate Polymers 112, 195-202. https://doi.org/10.1016/j.carbpol.2014.05.081
Zhang, C.-w., Nair, S. S., Chen, H., Yan, N., Farnood, R., and Li, F.-y. (2020). “Thermally stable, enhanced water barrier, high strength starch bio-composite reinforced with lignin containing cellulose nanofibrils,” Carbohydrate Polymers 230, article 115626. https://doi.org/10.1016/j.carbpol.2019.115626
Zhu, X., Hou, X., Ma, B., Xu, H., and Yang, Y. (2019). “Chitosan/gallnut tannins composite fiber with improved tensile, antibacterial and fluorescence properties,” Carbohydrate Polymers 226, article 115311. https://doi.org/10.1016/j.carbpol.2019.115311
Article submitted: June 29, 2026; Peer review completed: August 22, 2026; Revised version received and accepted: October 20, 2026; Published: November 1, 2026.
DOI: 10.15376/biores.21.4.12121-12138