Abstract
Ring-porous hardwoods contain marked anatomical differences between earlywood and latewood that can produce heterogeneous hygroscopic deformation. This exploratory study monitored growth-ring-scale hygroscopic deformation in one elm (Ulmus pumila L.) specimen using stereomicroscope-based two-dimensional digital image correlation (2D-DIC), while time-domain nuclear magnetic resonance (TD-NMR) measurements on four companion specimens were used to estimate moisture content at corresponding adsorption times. Tangential and radial displacement fields evolved progressively and remained spatially heterogeneous during adsorption. Local profiles at an earlywood position and a latewood position showed different responses, but these differences were interpreted as local deformation heterogeneity because the two positions experienced different boundary conditions. After 120 h, mean moisture content reached 25.0%, whereas median tangential and radial Green-Lagrangian swelling strains reached 0.0316 and 0.0169, respectively. In the monitored DIC specimen, tangential strain exceeded radial strain at all investigated time points, while additional strain increments were relatively small from 22 to 120 h, during which the companion specimens continued to absorb moisture. These results demonstrate transverse swelling anisotropy together with growth-ring-scale spatial heterogeneity and provide a material basis for assessing moisture-related dimensional stability and anatomical orientation in elm wood products.
Download PDF
Full Article
Transverse Hygroscopic Swelling of Elm Earlywood and Latewood and its Implications for Wood Product Design
Jia Liu,a Zheyu Li,b Bojun Zhang,a Wenjing Liu,b and Minghui Zhang b,*
Ring-porous hardwoods contain marked anatomical differences between earlywood and latewood that can produce heterogeneous hygroscopic deformation. This exploratory study monitored growth-ring-scale hygroscopic deformation in one elm (Ulmus pumila L.) specimen using stereomicroscope-based two-dimensional digital image correlation (2D-DIC), while time-domain nuclear magnetic resonance (TD-NMR) measurements on four companion specimens were used to estimate moisture content at corresponding adsorption times. Tangential and radial displacement fields evolved progressively and remained spatially heterogeneous during adsorption. Local profiles at an earlywood position and a latewood position showed different responses, but these differences were interpreted as local deformation heterogeneity because the two positions experienced different boundary conditions. After 120 h, mean moisture content reached 25.0%, whereas median tangential and radial Green-Lagrangian swelling strains reached 0.0316 and 0.0169, respectively. In the monitored DIC specimen, tangential strain exceeded radial strain at all investigated time points, while additional strain increments were relatively small from 22 to 120 h, during which the companion specimens continued to absorb moisture. These results demonstrate transverse swelling anisotropy together with growth-ring-scale spatial heterogeneity and provide a material basis for assessing moisture-related dimensional stability and anatomical orientation in elm wood products.
DOI: 10.15376/biores.21.4.12088-12103
Keywords: Digital image correlation; Earlywood; Elm; Hygroscopic swelling; Latewood
Contact information: a: School of Design, Inner Mongolia Arts University, Hohhot 011500, China; b: College of Materials Science and Art Design, Inner Mongolia Agricultural University, Hohhot 010018, China; *Corresponding author: [email protected]
INTRODUCTION
Wood is dimensionally responsive to changes in ambient humidity because water sorbed by the cell wall alters its internal structure. Adsorption therefore causes swelling and desorption causes shrinkage, with the magnitude of dimensional change strongly dependent on anatomical direction. Radial and tangential movement accounts for most of the transverse response, whereas longitudinal movement is comparatively small. Sorption history further complicates this behavior because adsorption/desorption and swelling/shrinkage do not follow identical paths (Patera et al. 2013; Ouyang et al. 2022). Dynamic exposure to changing relative humidity also produces time-dependent moisture responses (Yang et al. 2023). In wood products, such directional and time-dependent movement becomes important when adjacent regions or connected components are required to deform compatibly, because restraint can promote warping, cracking, or loss of fit.
The problem is particularly relevant at the growth-ring scale, where neighboring tissues can differ substantially in cell dimensions, wall fraction, density, and moisture response while remaining mechanically continuous. In ring-porous hardwoods, the contrast between vessel-rich earlywood and denser latewood creates a pronounced anatomical gradient within a single growth ring. Full-field measurements on Norway spruce, which is a conifer, have shown clear intra-ring variation in transverse swelling (Lanvermann et al. 2014), and three-dimensional digital image correlation (3D-DIC) has resolved different moisture-induced strain fields among earlywood and latewood tissues in red oak (Garcia et al. 2020). Ouyang et al. (2022) likewise reported differences in swelling/shrinkage and hysteresis among earlywood, latewood, and intact growth-ring regions of Catalpa bungei. More recent studies have identified moisture-dependent contrasts between earlywood and latewood in Chinese fir (Sun et al. 2024) and distinct cyclic moisture-sorption responses in southern pine (Luo et al. 2026). Together, these findings indicate that deformation measured at one anatomical position cannot automatically be treated as an unconstrained intrinsic property of that tissue; local response is also influenced by the surrounding growth-ring structure.
Elm (Ulmus pumila L.) is a representative ring-porous hardwood that is used extensively in furniture and woodcraft in northern China. Its marked earlywood-latewood contrast makes it well suited to the study of growth-ring-scale moisture deformation. While Liu et al. (2023) characterized drying-induced deformation, the present study focuses on the time-dependent evolution of tangential and radial swelling during moisture adsorption within an intact growth-ring structure. This distinction is relevant because moisture adsorption and desorption can exhibit hysteretic behavior (Patera et al. 2013; Ouyang et al. 2022). More specifically, the present study provides quantitative information on the temporal evolution of transverse swelling anisotropy. In the monitored DIC specimen, the ratio of median tangential to radial strain ranged from 1.62 at 2 h to 1.33 at 6 h and reached 1.87 at 22 h and 120 h. Together with the full-field displacement maps and fixed earlywood–latewood-position profiles, these results characterize directional swelling and spatial deformation heterogeneity during adsorption. Because the deformation measurements were obtained from one specimen, the findings are interpreted as exploratory observations rather than generalized tissue-specific swelling properties.
Conventional techniques, using equipment such as extensometers, dial gauges, and resistance strain gauges are suitable for measuring bulk dimensional change but provide limited information about local deformation within heterogeneous wood tissues. Digital image correlation avoids direct mechanical contact with the measured surface and provides spatially resolved displacement and strain fields. Its applicability to wood has been demonstrated for drying and hygroscopic deformation at several structural scales (Kwon and Hanna 2010; Joffre et al. 2016; Garcia et al. 2020, 2023). For elm, combining DIC with TD-NMR offers a useful separation of measurement functions: DIC records the spatial development of deformation on the observed surface, whereas TD-NMR provides an independent measure of the time-dependent moisture state of companion specimens. This combination makes it possible to compare the progression of deformation with moisture uptake without assuming that local earlywood and latewood positions share identical boundary conditions.
In the present study, elm (Ulmus pumila L.) was examined during moisture adsorption using DIC, stereomicroscopic imaging, and TD-NMR. The objectives were to characterize the temporal evolution of tangential and radial displacement and swelling strain at the growth-ring scale, to identify spatial heterogeneity associated with earlywood and latewood positions, and to compare the deformation response with time-matched moisture content. The measured local responses are interpreted within the mechanically continuous growth-ring structure rather than as direct, independent measurements of intrinsic earlywood and latewood swelling. The resulting transverse anisotropy and spatial heterogeneity are further considered in relation to moisture-related dimensional stability, with emphasis on material-level implications for component orientation, dimensional allowance, and moisture conditioning rather than direct manufacturing criteria.
EXPERIMENTAL
Sample Preparation
Elm wood (Ulmus pumila L.) was obtained from a single approximately 40-year-old tree grown in the Taipusi Banner Forest Farm, Xilin Gol City, Inner Mongolia, China. The diameter at breast height (DBH) was approximately 280 mm. One disk approximately 30 mm thick was collected from the stem at breast height. All five experimental specimens, including one specimen for DIC measurements and four companion specimens for TD-NMR measurements, were prepared from this disk. Consequently, the specimens shared the same biological source and were not considered independent biological replicates. Immediately after collection, the disk was wrapped in plastic film and stored in a refrigerator at approximately 4 °C for 6 days before specimen preparation to minimize moisture loss.
Specimens with dimensions of 12 (T) × 12 (R) × 20 (L) mm³ were prepared along the radial direction of the disk (Fig. 1). The specimen edges were oriented along the tangential (T), radial (R), and longitudinal (L) anatomical directions of the wood. The 12 × 12 mm² transverse surface was used as the observation surface for DIC measurements, with the radial direction extending across the growth-ring boundaries. The same anatomical orientation and specimen dimensions were used for the four TD-NMR companion specimens. The specimen dimensions were selected according to the combined requirements of the TD-NMR measurement and growth-ring-scale DIC analysis rather than a specific standardized specimen size. The available sample space of the TD-NMR system imposed a dimensional limitation, and the longitudinal dimension of 20 mm was selected to ensure compatibility with the measurement configuration. The same specimen geometry was used for the DIC specimen and the four TD-NMR companion specimens. The radial dimension of 12 mm retained two consecutive complete growth rings on the transverse observation surface because the average growth-ring width was approximately 6 mm. Each growth ring included an earlywood region approximately 1.25 mm wide and a latewood region approximately 4.75 mm wide. The transverse surface was polished under ambient laboratory conditions to provide a smooth imaging surface; temperature and relative humidity during this short preparation step were not independently recorded. The earlywood–latewood boundaries were preserved for local deformation analysis. After surface preparation, all specimens were oven-dried at 103 ± 2 °C until constant mass was reached. The oven-drying duration was the actual drying duration, whereas constant mass was determined based on the actual weighing interval and mass-change criterion. The oven-dry state was used as the common initial reference state for subsequent moisture adsorption measurements.
Moisture Sorption Experiment and Specimen Allocation
A total of five elm specimens were prepared for the moisture sorption experiment. Initially, all specimens were oven-dried in a drying oven (DHG-9070A, Shanghai Yiheng Scientific Instrument Co., Ltd., Shanghai, China) at 103 ± 2 °C until reaching a constant mass to obtain the oven-dry state. Subsequently, the specimens were placed in a constant temperature and humidity chamber (SH-100, Suzhou Sanqing Instrument Co., Ltd., Suzhou, China) maintained at 26 ± 1 °C and 87 ± 1% relative humidity (RH) for moisture sorption.
The DIC specimen and the four TD-NMR companion specimens were conditioned together in the same temperature- and humidity-controlled chamber during moisture adsorption. During the moisture sorption process, one specimen was selected for continuous deformation monitoring using digital image correlation (DIC). The specimen was vertically positioned beneath a stereomicroscope, and sequential images were continuously acquired to record the evolution of surface deformation. The image acquisition interval was set at one image every 10 s to capture the time-dependent displacement and strain evolution during moisture sorption.
The remaining four companion specimens were prepared from adjacent growth-ring regions of the same wood material and exposed to the same temperature and relative humidity conditions as the specimen used for DIC measurement. These specimens were used for time-domain nuclear magnetic resonance (TD-NMR) measurements at the selected sorption times. The same four companion specimens were used for TD-NMR measurements at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h. At each selected time point, the specimens were measured individually, and the resulting moisture-content values were summarized as the mean ± standard deviation (n = 4).
The DIC experiment was conducted on a single specimen without independent biological replication of the deformation measurements. The spatial correlation subsets and displacement profiles obtained from this specimen were treated as measurements within the same specimen rather than independent biological replicates. Accordingly, the present study was designed as an exploratory case study to characterize the spatial and temporal evolution of hygroscopic deformation in the monitored specimen.
It should be noted that the DIC measurements were performed on a single specimen, whereas the TD-NMR results represent the moisture response of four companion specimens. The DIC results are interpreted as specimen-specific observations of hygroscopic deformation.
Fig. 1. Schematic diagram of the test specimen
Full-field Deformation Measurement Using Digital Image Correlation
The digital image correlation (DIC) measurement was performed at 26 ± 1 °C and 87 ± 1% relative humidity. During moisture sorption, the specimen was vertically positioned beneath a stereomicroscope (SMZ-171, Motic, Xiamen, China), and the transverse surface containing two complete growth rings was recorded at 10-s intervals. The exposure setting was fixed at 92, and grayscale images were acquired at a resolution of 2048 × 1536 pixels. A 250-μm calibration scale was used to convert image coordinates to physical dimensions.
To ensure reliable image correlation analysis, the illumination conditions were maintained constant throughout the experiment to minimize intensity fluctuations. Prior to DIC measurement, the transverse surface was finely polished to improve image clarity, and the natural anatomical texture of the wood was used as the grayscale pattern for DIC analysis (Liu et al. 2023). The acquired images were subsequently used for displacement tracking and strain field reconstruction during the hygroscopic deformation process (Garcia et al. 2023).
The natural anatomical features of the polished transverse surface provided grayscale contrast for DIC tracking without applying an artificial speckle pattern. Illumination was maintained constant to reduce intensity variations during image acquisition. However, an independent quantitative validation of pattern stability during moisture adsorption was not available, and possible changes in grayscale features may have contributed to correlation uncertainty.
The region of interest (ROI) for full-field DIC analysis was defined on the transverse surface containing the two complete growth rings shown in Fig. 1. The specimen background outside the wood surface was excluded, and the same anatomical area was tracked throughout the moisture-sorption sequence. The image acquired in the initial oven-dry state immediately before moisture adsorption was used as the reference configuration (t = 0) for all subsequent DIC calculations.
Although images were continuously acquired at 10-s intervals throughout the 120-h adsorption experiment, only nine images corresponding to adsorption times of 2, 4, 6, 8, 10, 14, 22, 40, and 120 h were selected for quantitative DIC analysis. Together with the initial oven-dry reference image (t = 0), these images constituted the image set used for the reported DIC calculations. Image selection was based on the specified adsorption time points rather than processing the complete acquired image sequence.
The deformation analysis was performed using Ncorr (version [verified version], open-source 2D digital image correlation software, Georgia Institute of Technology, Atlanta, GA, USA). The DIC analysis was performed using Ncorr with a subset radius of 25 pixels and a subset spacing setting of 4, corresponding to a 5-pixel interval between adjacent subset centers. The displacement fields were calculated using the inverse compositional Gauss–Newton algorithm with biquintic B-spline interpolation. The convergence tolerance was set to 1 × 10⁻⁶, with a maximum of 50 iterations. Local displacement gradients were estimated using least-squares plane fitting with a strain radius of 7. The Green-Lagrangian strain components were obtained directly from the Ncorr full-field strain analysis, without additional logarithmic strain transformation or virtual-gauge calculations.
Each selected image was correlated with the initial oven-dry reference image using Ncorr to obtain the tangential and radial displacement fields at the corresponding adsorption time. Thus, the displacement of a material point at a given sorption time represents its change in position relative to the corresponding position in the initial oven-dry configuration. A displacement value of zero denotes no detected in-plane displacement relative to the initial reference image, whereas positive and negative values indicate movement in opposite directions within the image plane according to the defined coordinate system. A zero displacement value does not independently establish the absence of measurement noise or out-of-plane motion. The sign of displacement therefore indicates movement direction and should not by itself be interpreted as swelling or shrinkage. The resulting tangential and radial displacement fields are presented in Figs. 2 and 3.
Correlation with the common reference image enabled consistent comparison of the selected deformation states. However, this procedure does not independently account for possible imaging-system drift. A separate registration or drift-correction procedure could not be verified from the available processing records. Therefore, the potential contribution of residual drift to the measured displacement and strain fields remains unquantified.
After the full-field displacement calculation, two fixed local profiles, M and N, were extracted from the calculated displacement fields according to the visible anatomical positions. Profile M was located within an earlywood region near the specimen edge, whereas profile N was located within a latewood region in the interior of the specimen, as indicated in Figures 2(b) and 3(b). Their anatomical positions were identified by comparison with Figures 2(a) and 3(a). M and N therefore represent fixed profile locations within the full-field ROI rather than separate DIC regions of interest. The same profile positions and the same initial reference configuration were used throughout the complete sorption sequence. Displacement profiles at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h were extracted for subsequent comparison.
The Green–Lagrangian strain tensor was used to characterize the hygroscopic deformation of the monitored specimen relative to the initial oven-dry reference configuration. The tangential and radial swelling strains corresponded to the normal strain components Eₓₓ and Eᵧᵧ, respectively, where the x- and y-directions represented the tangential and radial anatomical directions.
The Green–Lagrangian strain tensor was defined as follows,
E = ½(FᵀF − I) (1)
where E is the Green–Lagrangian strain tensor, F is the deformation gradient tensor, and I is the identity tensor. The tangential and radial swelling strains were defined as εT = Eₓₓ and εR = Eᵧᵧ, respectively. No additional logarithmic strain transformation was performed, and the tangential and radial strains were not calculated from predefined virtual-gauge lengths; instead, the Green–Lagrangian strain components obtained directly from Ncorr were used for subsequent spatial statistical analysis.
At each selected adsorption time, the full-field strain data were exported from Ncorr for spatial statistical analysis. The valid strain values within the defined region of interest (ROI) were used to determine the median, maximum, and minimum values in the tangential and radial directions. These statistics characterize spatial variations within the monitored DIC specimen rather than independent biological replicates.
Determination of Moisture Content by TD-NMR
Time-domain nuclear magnetic resonance measurements were performed using a Minispec mq20 spectrometer (Bruker, Billerica, MA, USA). The four companion specimens were subjected to the same moisture sorption conditions as the specimen used for DIC measurement. At each selected sorption time, transverse relaxation decay signals were acquired from each companion specimen using a Carr–Purcell–Meiboom–Gill pulse sequence under identical acquisition conditions. The original instrument-setting records available for this revision did not retain the exact echo spacing, number of echoes and scans, repetition time, or NMR acquisition temperature; these parameters could therefore not be independently verified.
The transverse relaxation decay curves were fitted using a bi-exponential model in OriginPro 2020 (OriginLab Corporation, Northampton, MA, USA) as follows,
(2)
where S(t) is the NMR signal intensity at decay time t; A₁ and A₂ are the signal amplitudes of the two resolved water components; and T₂,₁ and T₂,₂ are their corresponding transverse relaxation times.
The total NMR signal amplitude was calculated as
(3)
Because the total CPMG signal amplitude is proportional to the number of mobile hydrogen nuclei in the specimen, water mass was obtained from the calibration relationship
(4)
where k and b are calibration coefficients established under identical acquisition conditions.
The NMR-derived moisture content was calculated as,
(5)
where m₀ is the oven-dry mass of the specimen. The NMR-derived moisture content at each selected sorption time was expressed as the mean ± standard deviation of four companion specimens (n = 4). Measurements were conducted at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h. The standard deviations ranged from 0.43 to 1.32 percentage points, reflecting the variability in moisture content among the four companion specimens under the corresponding adsorption conditions. These values characterize the time-dependent mean moisture state of the companion specimens and should not be interpreted as the exact instantaneous moisture content of the DIC specimen.
RESULTS AND DISCUSSION
Evolution of Tangential Displacement and Local Earlywood–Latewood Response during Moisture Sorption
DIC displacement describes the movement of tracked surface points relative to their initial positions and therefore retains information on both the magnitude and spatial direction of local movement. For this reason, displacement in millimeters was retained in Figs. 2 and 3 to characterize the spatial and temporal evolution of the deformation field. Local deformation was quantified separately using the Green–Lagrangian strain components obtained from Ncorr, as described earlier and statistically summarized in Table 1. Figure 2(a) presents the transverse anatomical morphology of the investigated surface, in which earlywood and latewood regions can be identified within two consecutive growth rings. Figure 2(b) shows the tangential displacement field after 2 h of moisture sorption. At this time, the displacement magnitude varied across the investigated surface, indicating a spatially non-uniform tangential displacement response.
Figure 2(c) presents the tangential displacement fields at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h. Comparison of these fields shows that the magnitude of tangential displacement progressively increased with moisture-sorption time, while spatial differences remained across the investigated growth-ring surface. Thus, Figure 2(c) directly demonstrates both the temporal evolution and spatial heterogeneity of tangential displacement during moisture adsorption.
The progressive increase in tangential displacement is consistent with hygroscopic expansion of the cell-wall structure during moisture adsorption. The persistent spatial differences in Fig. 2(c), however, show that this response was not uniform across the natural growth-ring structure (Almeida et al. 2014; Lanvermann et al. 2014).
The negative displacement values in Fig. 2 arise from the DIC coordinate definition. They indicate movement direction relative to the reference configuration and should not be interpreted as shrinkage. Swelling deformation was assessed using the full-field strain data obtained from Ncorr rather than the sign of an individual displacement value.
Fig. 2. Evolution of tangential displacement during moisture sorption. (a) Initial transverse morphology showing earlywood and latewood; (b) full-field tangential displacement after 2 h, with fixed profile positions M and N; (c) full-field displacement at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h; (d) local tangential displacement profiles at earlywood position M; and (e) local tangential displacement profiles at latewood position N
Figures 2(d) and 2(e) show local tangential displacement profiles at positions M and N, respectively. Both profiles evolved with sorption time, but they followed different local trajectories. Because M lies in earlywood near the specimen edge whereas N lies in interior latewood, the two positions experience different local boundary conditions. Their differences therefore represent local growth-ring-scale deformation heterogeneity and cannot be treated as independent quantitative measures of intrinsic earlywood and latewood swelling.
Moisture adsorption expands the cell-wall polymer matrix as water interacts with hydroxyl-rich constituents (Cave 1978). Variations in cell-wall proportion and anatomical organization can therefore contribute to spatially heterogeneous deformation. In the present experiment, however, the DIC data do not isolate these factors independently; the displacement field should be interpreted as the integrated response of anatomy, moisture uptake, and structural constraint.
Comparison of Figs. 2(d) and 2(e) at the selected sorption times shows that the local displacement profiles at positions M and N evolved differently during adsorption, and the differences became more apparent at the intermediate and later stages. Because the NMR-derived moisture contents represent specimen-average values obtained from the companion specimens, these local displacement differences cannot be assigned to a specific moisture-content threshold of either earlywood or latewood.
Earlywood and latewood form a continuous growth-ring structure rather than mechanically independent domains. Differential local swelling can therefore be accommodated through deformation compatibility and constraint between adjacent regions (Rafsanjani et al. 2012; Ouyang et al. 2022). The present M–N comparison supports this integrated growth-ring interpretation but does not quantify interfacial stress.
Overall, tangential displacement increased with sorption time and remained spatially heterogeneous. The different M and N trajectories are interpreted as local growth-ring-scale responses rather than intrinsic tissue-specific swelling properties.
Radial Displacement Behavior and Local Earlywood–latewood Deformation During Moisture Sorption
Figure 3(a) presents the initial transverse morphology of the investigated surface, while Fig. 3(b) shows the radial displacement field after 2 h of moisture sorption. Figure 3(c) presents the temporal evolution of the radial displacement field at the selected sorption times. Positive and negative displacement values indicate movement in opposite directions relative to the defined radial coordinate system and therefore describe displacement direction rather than swelling or shrinkage by themselves.
As shown in Fig. 3(c), the radial displacement field exhibited clear temporal evolution during moisture sorption. During the earlier stages of adsorption, regions with both positive and negative radial displacement were present within the analyzed surface. In particular, the upper part of the investigated surface predominantly showed displacement in the negative radial direction, whereas the lower part showed displacement in the positive radial direction. With increasing sorption time, both the magnitude and spatial distribution of radial displacement progressively changed. These observations demonstrate that radial deformation was spatially heterogeneous during moisture adsorption. The radial displacement sign is defined relative to the initial oven-dry reference image, with positive and negative values indicating opposite directions of in-plane movement along the radial axis. The observed sign reversal represents a change in local displacement direction and should not be interpreted directly as a transition between swelling and shrinkage. Possible contributions from local geometric constraints and specimen motion cannot be excluded.
The temporal evolution in Fig. 3(c) is consistent with progressive hygroscopic expansion during moisture adsorption. Because the natural growth-ring structure is anatomically heterogeneous, radial movement varied across the observed surface rather than evolving uniformly (Patera et al. 2013; Fu et al. 2021). Differences in cellular structure and cell-wall proportion provide a plausible basis for this spatial variation, although these anatomical contributions were not independently measured.
Figures 3(d) and 3(e) show local radial displacement profiles at positions M and N. Both evolved with sorption time, but the two profiles differed. As in the tangential analysis, the positions were subject to different local boundary conditions; therefore, the M–N differences should be interpreted as local growth-ring-scale responses rather than as direct measurements of intrinsic earlywood–latewood radial swelling differences.
Fig. 3. Evolution of radial displacement during moisture sorption. (a) Initial transverse morphology showing earlywood and latewood; (b) full-field radial displacement after 2 h, with fixed profile positions M and N; (c) full-field radial displacement at 2, 4, 6, 8, 10, 14, 22, 40, and 120 h; (d) local radial displacement profiles at earlywood position M; and (e) local radial displacement profiles at latewood position N. Panels (d) and (e) correspond to the same chronological sorption sequence shown in panel (c). Displacement signs indicate in-plane movement relative to the initial oven-dry reference image; positive and negative values denote opposite directions along the defined radial axis
Because earlywood and latewood are anatomically connected, local deformation occurs within the constraint of the surrounding growth-ring structure. Differential hygroscopic deformation among adjacent tissues can produce mechanically constrained responses (Rafsanjani et al. 2012; Ouyang et al. 2022). However, the earlywood–latewood boundary was not analyzed as an independent region and interfacial stress was not measured; the present data therefore do not quantify a specific interfacial constraint mechanism.
Wood rays were naturally present within the analyzed transverse surface and were not separately segmented. Their contribution is therefore included in the measured radial displacement field, which represents the integrated response of earlywood, latewood, interfaces, and rays. Because ray-specific regions were not analyzed, the individual contribution of rays to radial deformation and transverse anisotropy cannot be quantified from the present data.
Overall, radial displacement evolved continuously and remained spatially heterogeneous across the growth-ring surface. The M and N profiles also followed different temporal trajectories, but the measured field represents the integrated response of all anatomical features within the analyzed area.
Time-matched Evolution of Hygroscopic Swelling Strain and NMR-derived Moisture Content
Table 1 summarizes the tangential and radial Green-Lagrangian swelling strains obtained from the Ncorr full-field strain analysis, their median-based anisotropy ratio, and the time-matched NMR-derived moisture content. At each adsorption time, the median, maximum, and minimum strain values were calculated from the valid spatial strain observations within the defined DIC region of interest. These statistics represent spatial strain variations within the monitored specimen rather than independent biological replicates. The NMR-derived moisture-content values represent the mean ± standard deviation of four companion specimens. At 120 h, the median tangential and radial Green-Lagrangian strains reached 0.0316 and 0.0169, respectively.
At 2 h, the median tangential and radial swelling strains were 0.0076 and 0.0047, respectively, giving a tangential-to-radial ratio of 1.62. At 22 h, the corresponding strains were 0.0309 and 0.0165 and the ratio was 1.87. At 120 h, the strains reached 0.0316 and 0.0169, while the ratio remained 1.87. The present data therefore show that tangential swelling exceeded radial swelling throughout the investigated adsorption process, consistent with transverse swelling anisotropy reported for wood (Patera et al. 2013; Ouyang et al. 2022).
During the initial sorption stage, the tangential-to-radial strain ratio fluctuated, decreasing from 1.62 at 2 h to 1.37 at 4 h and 1.33 at 6 h before increasing to approximately 1.87 by 22 h. The early fluctuation indicates that tangential and radial deformation did not evolve proportionally with time. Because the NMR measurements represent specimen-average moisture content rather than spatial moisture distributions, the present data do not identify a local moisture mechanism for this transient variation.
The median tangential strain increased from 0.0120 at 6 h to 0.0232 at 8 h. Because the original pointwise Ncorr strain-field data were not retained, the contribution of measurement or processing effects to this pronounced change could not be independently assessed. This increase is therefore reported as an observed change in the monitored specimen, without attributing it to a specific transient deformation mechanism.
During the later stage of adsorption, moisture uptake and deformation no longer increased proportionally. From 22 to 120 h, the NMR-derived mean moisture content of the companion specimens increased from 18.9% to 25.0%, whereas median tangential strain increased only from 0.0309 to 0.0316 and median radial strain from 0.0165 to 0.0169. Between 22 and 120 h, the median tangential and radial strains in the monitored DIC specimen increased only slightly, while the mean moisture content measured in the four companion specimens continued to rise. Because these quantities were measured on different specimens and neither an independent equilibrium criterion nor quantified DIC strain uncertainty was available, these observations should be interpreted only as a time-matched trend. They do not establish a true strain plateau, moisture equilibrium, or a specimen-specific mechanism relating moisture uptake to swelling.
The spatial DIC fields further showed that local displacement was not uniform across the growth-ring surface. The M and N profiles evolved differently during adsorption, but these local observations are distinct from the specimen-level strain statistics in Table 1. Accordingly, Table 1 is not used to infer separate quantitative earlywood and latewood swelling strains.
Table 1. Tangential and Radial Swelling Strains and NMR-derived Moisture Contents of Elm at Different Moisture Sorption Times
DESIGN IMPLICATIONS FOR HYGROSCOPIC DIMENSIONAL STABILITY
The results have three material-level implications for wood-product design: directional swelling anisotropy (Table 1), relatively small late-stage strain increments, and spatial heterogeneity within growth rings (Figs. 2 and 3). These findings are used to discuss component orientation, dimensional allowance, moisture conditioning, and local dimensional compatibility; they are not direct manufacturing criteria. The following discussion distinguishes directly observed specimen-level responses from potential design implications, which require independent validation before being applied as product-level recommendations.
Component Orientation and Dimensional Allowance
The quantitative results in Table 1 show that tangential swelling strain remained greater than radial strain throughout adsorption. This directional difference indicates that component orientation is relevant when moisture-induced movement and compatibility with adjacent components are considered. Dimensional allowance should therefore not be assumed to be equivalent in the radial and tangential directions. The present strain values, however, cannot be converted directly into product clearances or manufacturing tolerances because these also depend on component size, restraint, moisture range, and product configuration.
Implications for Moisture Conditioning
The time-matched results presented earlier indicate that, from 22 to 120 h, mean moisture content continued to increase while additional tangential and radial strain increments became small. For dimension-sensitive processing and assembly, this supports consideration of the material moisture state when dimensional inspection, fitting, or assembly depends on stability. The present data do not define a universal equilibrium criterion, conditioning duration, or target moisture content for manufacturing.
Moisture conditioning under environmental conditions relevant to subsequent processing or service may reduce further dimensional change after machining or assembly. Dimensional inspection performed before moisture-induced deformation has sufficiently stabilized may not represent the later dimensional state. These observations are consistent with the practical importance of moisture conditioning before dimension-sensitive processing. However, the present experiment did not establish when dimensional equilibrium was reached, and specific conditioning requirements should be determined independently at the component or product scale.
Effects of Earlywood–latewood Heterogeneity on Local Deformation
The DIC results in Figs. 2 and 3 show that moisture-induced deformation was spatially heterogeneous across the transverse surface. Locations within the same growth-ring structure followed different displacement trajectories, demonstrating that specimen-level directional strain values do not capture all local deformation heterogeneity.
This heterogeneity may be relevant where local deformation is mechanically constrained, because adjacent anatomical regions can respond differently to moisture. However, the present study did not directly test finished products, joints, or laminated assemblies. The findings should therefore be treated as material-level information on local dimensional compatibility rather than as direct product-design recommendations.
CONCLUSIONS
1. In the single elm specimen monitored by DIC, the tangential and radial displacement fields evolved progressively during moisture adsorption and remained spatially heterogeneous across the growth-ring surface. The M and N profiles followed different temporal trajectories; given their different local boundary conditions, these differences are interpreted as local deformation patterns rather than intrinsic tissue-specific swelling properties.
2. At 120 h, the mean moisture content measured by TD-NMR in the four companion specimens reached 25.0%, whereas the median tangential and radial Green-Lagrangian strains in the monitored DIC specimen reached 0.0316 and 0.0169, respectively. Tangential strain exceeded radial strain at all investigated time points in this specimen, while the additional strain increments from 22 to 120 h were relatively small. These values represent observations under the experimental conditions of this study rather than population-level estimates.
3. The observed transverse anisotropy and spatial heterogeneity provide exploratory, specimen-level information relevant to moisture-related dimensional stability and anatomical orientation in elm wood. Because the DIC analysis was conducted on a single specimen and the NMR measurements were performed on four companion specimens, further studies using independent DIC specimens are required to assess the reproducibility and broader applicability of these findings. The present results should not be interpreted as universal properties of elm wood or as direct manufacturing criteria.
ACKNOWLEDGMENTS
This work was supported by the Scientific Research Start-up Fund of Inner Mongolia Arts University (Grant No. KYQDJ05), the Research Innovation Team Development Program of Inner Mongolia Arts University (Grant No. 24CXTD04), the Natural Science Foundation of Inner Mongolia Autonomous Region of China (Grant No. 2023MS03027), and the National Natural Science Foundation of China (Grant Nos. 32560334, 31860185, and 31160141).
Declaration of Competing Interest
The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.
Author Contributions
J.L.: Data curation; software; formal analysis; funding acquisition; investigation; methodology; project administration; validation; writing – original draft; writing – review & editing. Z.Y.L.: Writing – review & editing. J.B.Z.: Investigation. W.J.L.: Supervision. M.H.Z.: Funding acquisition; methodology; project administration; resources; writing – original draft; writing – review & editing.
Data Availability
The reported results and supporting descriptions are provided in this article. The original pointwise Ncorr strain-field exports, time-specific validity masks, and original NMR calibration dataset were not retained and are therefore unavailable for independent reanalysis.
REFERENCES CITED
Almeida, G., Huber, F., and Perré, P. (2014). “Free shrinkage of wood determined at the cellular level using an environmental scanning electron microscope,” Maderas Cienc. Tecnol. 16, 187-198. https://doi.org/10.4067/S0718-221X2014005000015
Cave, I. D. (1978). “Modelling moisture-related mechanical properties of wood. Part I: Properties of the wood constituents,” Wood Sci. Technol. 12, 75-86. https://doi.org/10.1007/BF00390012
Fu, Z., Weng, X., Gao, Y., and Zhou, Y. (2021). “Full-field tracking and analysis of shrinkage strain during moisture content loss in wood,” Holzforschung 75, 436-443. https://doi.org/10.1515/hf-2020-0086
Garcia, R. A., Rosero-Alvarado, J., and Hernández, R. E. (2020). “Full-field moisture-induced strains of the different tissues of tamarack and red oak woods assessed by 3D digital image correlation,” Wood Sci. Technol. 54, 139-159. https://doi.org/10.1007/s00226-019-01145-5
Garcia, R. A., Rosero-Alvarado, J., and Hernández, R. E. (2023). “Moisture-induced strains in earlywood and latewood of mature and juvenile woods in jack pine from 3D-DIC measurements,” Wood Mater. Sci. Eng. 18, 570-579. https://doi.org/10.1080/17480272.2022.2056714
Joffre, T., Isaksson, P., Dumont, P. J. J., Rolland du Roscoat, S., Sticko, S., Orgéas, L., and Gamstedt, E. K. (2016). “A method to measure moisture induced swelling properties of a single wood cell,” Exp. Mech. 56, 723-733. https://doi.org/10.1007/s11340-015-0119-9
Kwon, O., and Hanna, R. (2010). “The enhanced digital image correlation technique for feature tracking during drying of wood,” Strain 46, 566-580. https://doi.org/10.1111/j.1475-1305.2008.00455.x
Lanvermann, C., Wittel, F. K., and Niemz, P. (2014). “Full-field moisture induced deformation in Norway spruce: Intra-ring variation of transverse swelling,” Eur. J. Wood Wood Prod. 72, 43-52. https://doi.org/10.1007/s00107-013-0746-8
Liu, J., Liu, W., Tan, R., Huang, W., Wang, B., Zhang, S., and Zhang, M. (2023). “Drying strain behavior of elm earlywood and latewood with digital image correlation method,” Dry. Technol. 41, 746-753. https://doi.org/10.1080/07373937.2022.2114492
Luo, D., Yang, T., Wang, L., and Mei, C. (2026). “Cyclic moisture sorption and moisture buffering response of earlywood and latewood of southern pine to sinusoidally changing relative humidity,” Wood Mater. Sci. Eng. 21, 612-622. https://doi.org/10.1080/17480272.2024.2439588
Ouyang, B., Yin, F., Li, Z., and Jiang, J. (2022). “Study on the moisture-induced swelling/shrinkage and hysteresis of Catalpa bungei wood across the growth ring,” Holzforschung 76, 711-721. https://doi.org/10.1515/hf-2021-0222
Patera, A., Derome, D., Griffa, M., and Carmeliet, J. (2013). “Hysteresis in swelling and in sorption of wood tissue,” J. Struct. Biol. 182, 226-234. https://doi.org/10.1016/j.jsb.2013.03.003
Rafsanjani, A., Derome, D., Wittel, F. K., and Carmeliet, J. (2012). “Computational up-scaling of anisotropic swelling and mechanical behavior of hierarchical cellular materials,” Compos. Sci. Technol. 72, 744-751. https://doi.org/10.1016/j.compscitech.2012.02.001
Sun, F., Li, R., Zhu, J., Peng, H., Li, Z., Jiang, J., Zhan, T., Cai, L., and Lyu, J. (2024). “Comparison analysis of moisture-dependent orthotropic elasticity between earlywood and latewood in Chinese fir using digital image correlation,” Ind. Crops Prod. 220, article 119185. https://doi.org/10.1016/j.indcrop.2024.119185
Yang, T., Mei, C., and Qian, S. (2023). “Dynamic moisture sorption and humidity response inside the wooden space to cyclical changing external relative humidity,” Wood Mater. Sci. Eng. 18, 1922-1932. https://doi.org/10.1080/17480272.2023.2204069
Article submitted: September 17, 2026; Peer review completed: October 17, 2026; Revised version received and accepted: October 19, 2026; Published: October 30, 2026.
DOI: 10.15376/biores.21.4.12088-12103